Foundry Sand Sieve Analysis: GFN, Grading and Cost

Foundry sand sieve analysis: a stack of wire-cloth test sieves with retained sand samples

Foundry sand sieve analysis is the single cheapest test that tells you why a mold bleeds gas, why bond demand crept up, or why one supplier’s “GFN 53” sand casts cleanly while another’s produces pinholes. It reduces a bulk sample to a particle-size distribution and one number — the AFS grain fineness number. This guide shows the exact arithmetic, why two sands with the same GFN can behave completely differently, and the cost of letting grading drift.

Everything below is built on the AFS 1106-00-S grain-fineness procedure, the ASTM E11 wire-cloth sieve specification that defines the test sieves, and measurement-traceability guidance from NIST metrology. Grain size is one input to casting quality — it interacts with permeability, bond, moisture and melt chemistry, topics covered more broadly in our руководство по литью металлов и литье в зелёные пески references. For the cost side, see our foundry sand reclamation analysis.

Foundry sand sieve analysis: a stack of wire-cloth test sieves with retained sand samples
Figure 1. A foundry sand sieve analysis starts with a weighed sample on a certified stack of ASTM E11 sieves.

1. What a Foundry Sand Sieve Analysis Actually Measures

A foundry sand sieve analysis answers one question: how much of the sample sits in each particle-size band? A dried, de-clayed sand sample — typically 50 g or 100 g — is placed on the top of a nest of sieves arranged coarse to fine. The stack is shaken for a fixed time. Each screen retains the grains too large to pass its opening. Weighing what each deck holds gives the percent retained, and those percentages are the distribution.

Two things come out of the same run. First, the full distribution curve: the shape tells you whether the sand is tightly graded (one narrow peak) or spread across many sizes. Second, a single summary value — the AFS grain fineness number (GFN) — computed by multiplying each sieve’s percent retained by a fixed multiplier and dividing the sum of products by the sum of percentages. The GFN is an estimate of average grain size in mesh terms. Crucially, as the Michigan geological survey notes, the GFN contains no information about the size distribution — a point this article returns to in Section 5.

In practice a foundry sand sieve analysis is run on washed system sand to strip clay and organic coatings that cement grains together. Comparing the washed screen analysis with the dried (unwashed) one reveals how much agglomeration is occurring in the system — a diagnostic that pairs directly with the foundry audit checklist and the control plan in our incoming inspection plan.

2. The Sieve Stack and the AFS GFN Formula

The test uses the U.S. standard (Tyler/ASTM E11) sieve series. Each sieve has a defined opening and a fixed AFS multiplier. The multiplier rises steeply for fine screens, which is why a small shift of mass into the fines pushes the GFN up sharply.

U.S. meshOpening (mm)AFS multiplier (1106)
63.360.03
121.680.05
200.840.10
300.590.20
400.420.30
500.2970.40
700.2100.50
1000.1490.70
1400.1051.00
2000.0741.40
2700.0532.00
Pan—3.00

The calculation is GFN = Σ(% retained × multiplier) ÷ Σ(% retained). Since the percentages sum to 100, the divisor is normally 100. Below is a worked foundry sand sieve analysis on a 100 g sample — every product is shown so you can reproduce it at the bench. This is the arithmetic behind the number your supplier quotes.

Mesh% retained on sieveProduct (% × multiplier)
600.00
1200.00
2000.00
3010.20
4082.40
502510.00
704020.00
1002014.00
14055.00
20011.40
27000.00
Pan00.00

Sum of products = 53.00; sum of retained = 100; therefore AFS GFN = 53.00 (reported as GFN 53). Note how the 70-mesh fraction (40% retained, product 20.00) and the 100-mesh fraction (20% retained, product 14.00) dominate the result. A verification of sieve calibration and sample mass belongs in the same measurement system discussed under NIST traceability.

3. How to Run a Foundry Sand Sieve Analysis at the Bench

A repeatable foundry sand sieve analysis follows a fixed sequence. Skip a step and the number drifts.

  • De-clay the sample. Wash the sand until the clay is removed; this is the same AFS clay-wash step used before a loss-on-ignition test.
  • Dry to constant mass. Oven-dry so moisture does not bias the weighed fractions.
  • Weigh the sample. Use 50 g or 100 g, recorded to 0.1 g.
  • Stack coarse to fine. Top screen coarsest, pan at the bottom; never invert the stack.
  • Shake for a fixed time. A mechanical shaker removes operator-to-operator variation.
  • Weigh each retained fraction. Record grams on each deck, convert to percent, apply multipliers.
  • Compute GFN and plot the curve. Track both the number and the distribution shape on every lot.

Consistency matters more than speed. A 2026 bench study notes that weighing the retained sand in place on each sieve — rather than brushing it onto a balance — avoids pushing grains into the next cut and keeps the certified weave inside tolerance. The same discipline applies to mold coating thickness control и core-making: the test is only as good as the sampling.

Foundry sand sieve analysis: precision balance weighing a retained sand fraction
Figure 2. Weighing each retained fraction to 0.1 g is where foundry sand sieve analysis accuracy is won or lost.

4. From Percent Retained to a Grading Curve

The distribution is more useful than the single GFN. Plot cumulative percent passing against sieve opening on a logarithmic axis and you get the grading curve. Its steepness and peak location explain behavior the GFN cannot:

  • Narrow (well-graded) sand. Most mass on two or three adjacent screens — high permeability, predictable bond demand, smoother finish.
  • Broad sand. Mass spread widely — more fines fill the voids, lowering permeability and raising bond demand.
  • Bimodal sand. Two peaks, typically a coarse one and a fines tail — often the fingerprint of reclamation drift or a blended incoming load.

The two sample distributions used in this article make the point concrete. Sand A is narrow and well-graded; Sand B carries a coarse peak plus a heavy fines tail. Both run through the same foundry sand sieve analysis method, and — as the next section shows — they produce almost identical GFN values.

5. Why Two Sands With the Same GFN Behave Differently

Here is the counter-intuitive result that makes foundry sand sieve analysis worth doing. The two 100 g samples below have GFN values within 0.4 of each other, yet their fines content — the fraction at 140 mesh and finer — differs by three times. That fines tail controls permeability and gas-evolution behavior far more than the average number does.

MetricSand A (narrow)Sand B (bimodal)Interpretation
GFN (AFS 1106)53.0052.60essentially identical
Fines at 140 mesh & finer6%18%3× more fines in B
50–100 mesh main fraction85%32%A concentrated in the sweet band
Illustrative permeability (AFS units)110372.9× lower in B
Predicted porosity-scrap rate1.2%3.1%2.6× higher in B

A buyer who specifies only “GFN 53” can legally receive either sand. In the mold, Sand B’s extra fines pack into the voids between coarse grains, cutting gas permeability roughly by 3×. The result shows up as gas porosity and pinholes, the exact defects graded in ASTM E446 reference radiographs. This is why a serious foundry sand sieve analysis reports the full distribution alongside the GFN, not the number alone — and why casting simulation fed with a single average grain size can mislead.

6. How Grading Drives Permeability, Bond Demand and Finish

Three casting outcomes trace directly to the distribution your foundry sand sieve analysis reveals.

Permeability and gas defects


Permeability is how readily gases escape the mold. Coarse, uniformly graded sand has large interconnected voids and high permeability. Fines plug those channels. When metal is poured — see the pouring-temperature window — binders and coatings generate gas that must exit before it is trapped at the metal/mold interface. Low-permeability Sand B raises the pinhole and blow risk captured in our пористость и усадка guide.

Bond demand and cost


Finer sand has more surface area per kilogram, so it needs more bentonite or resin to coat each grain. In this model the narrow sand needs about 5.72% bentonite while the bimodal sand needs 6.56% — a 0.84 percentage-point difference. On a 30,000 t/year green-sand system at $340/t for bentonite, that is $583,440 versus $669,528 per year: $86,088 of extra bond from grading drift alone.

Surface finish and shakeout


Finer grains generally produce a smoother as-cast surface, which is why литье по выплавляемым моделям и литье под давлением processes favor fine media. But at the green-sand end, too many fines hurt permeability and make shakeout harder. The art is choosing a narrow distribution at the fineness your surface spec needs, then holding it — the trade-off discussed in sand vs investment casting and on our sand casting service page. Sand grading also sets the tolerance stack on machined surfaces, so our CNC machining services start from the as-cast datum; tooling and изготовление литейных форм fix that datum, and our metal prototype casting route uses the same sieve discipline on short runs.

7. The Cost of Ignoring Grading Drift

Reclamation systems gradually accumulate fines; incoming sand lots vary. Without a routine foundry sand sieve analysis, the drift is invisible until scrap climbs. The model below prices a year of uncontrolled grading on a mid-size iron foundry making 85,000 ductile-iron parts (18 kg each) — the kind of component specified under ASTM A536.

Строка расходовControlled grading (A)Drifted grading (B)Difference
Bentonite (30,000 t system)$583,440$669,528$86,088
Porosity scrap (1.2% → 3.1%)$25,398$65,612$40,214
Total annual penalty——$126,302

A sieve-control program — three foundry sand sieve analysis runs per week, $22 labor each, $1,800/year sieve replacement and $1,200/year equipment amortization — costs about $6,432/year. Against a $126,302 penalty that is a 20× return and a payback of roughly 19 days. The economic case for testing is usually decided here, long before any metallurgical argument.

8. Writing a Grading Specification Buyers Can Enforce

A purchase order that says only “GFN 53” invites the two-sand problem above. Specify the distribution.

  • GFN target and tolerance. e.g. GFN 53 ± 3 per AFS 1106 on washed, dried sand.
  • Fines cap. e.g. max 8% total on 140 mesh and finer — the number that separates Sand A from B.
  • Main-band requirement. e.g. ≥ 60% retained cumulatively across 50–100 mesh.
  • Test standard. Name ASTM E11 sieves and the AFS 1106 method explicitly.
  • Sampling and reporting. Require a distribution table, not just the number, on every lot.
  • Re-test trigger. Any change of sand source or reclamation setting requires a fresh screen analysis.

Fold these fields into the supplier scorecard in our foundry audit checklist and the clay/LOI controls in sand reclamation. They also belong in the incoming-material section of a quality agreement — for that document set, see our методы контроля литья и core-making references.

9. Lab QA: Five Errors That Wreck a Sieve Result

A foundry sand sieve analysis is only as trustworthy as the bench technique behind it. The arithmetic is simple; the failures are almost always procedural. Here are the five errors that distort more GFN reports than any metallurgical variable, each with the control that removes it.

ErrorEffect on resultУправление
Sample not de-clayedClay cements grains; false coarse peakWash to AFS clay endpoint before screening
Under-dryingMoisture biases weighed fractionsDry to constant mass, cool in desiccator
Inconsistent shake timePoor separation, drifting percentagesMechanical shaker, fixed timer
Worn or damaged sieve clothOpenings out of ASTM E11 toleranceAnnual calibration, replace torn mesh
Brushing sand off the sieveForces grains to wrong deckWeigh retained in place, ultrasonic clean
Foundry sand sieve analysis: a mechanical sieve shaker with a certified sieve stack
Figure 3. A mechanical shaker and certified ASTM E11 cloth remove the two biggest variables in foundry sand sieve analysis: time and aperture.

Run a reference sand every week


The most effective control is a retained reference sample of known GFN. Run it through the same foundry sand sieve analysis procedure each week and plot the result on a control chart. If the reference drifts more than ±1 GFN, the problem is the test — sieve wear, shaker timing, balance calibration — not the sand. This separates measurement noise from real system-sand change before you re-bond or add new sand on a false signal. It is the same gauge-repeatability discipline used for dimensional inspection methods and written into a quality agreement.

Choose the right sample mass for the fineness


Sample mass is not arbitrary. Coarser sands need a larger test portion so that a single oversized grain does not swing a percentage point; fine sands can be run on 50 g. A 100 g portion is standard for the mesh series used here and keeps each retained fraction large enough to weigh accurately on a 0.1 g balance. Whichever mass you choose, hold it constant lot to lot — a foundry sand sieve analysis compared across different sample masses is not a valid trend, because the statistical weight of the coarse fraction changes with the total. Record the mass on the report alongside the GFN and the distribution.

Sample the system, not the truck top


System sand stratifies. A scoop from the top of a hopper or the crown of a delivery truck is not representative. Take multiple increments from a moving stream or across the pile, then split down to the test mass with a riffle splitter. Sampling error routinely exceeds the GFN tolerance itself, so a perfect bench test on a bad sample still misleads. Document the sampling point on every report so a trend can be traced back to its source — reclaimed sand, new sand addition, or a specific supplier lot.

Log the curve, not just the number


Store the full percent-retained vector for every foundry sand sieve analysis, not only the GFN. A rising fines tail with a flat GFN is an early warning of reclamation wear or carryover; you cannot see it in a single number. Over a season, that log becomes the evidence base for supplier negotiations and for tying sand condition to the porosity and surface results recorded in foundry audit records. It also closes the loop with the permeability and bond relationships developed in Sections 5 and 6, turning a routine sieve check into a predictive control.

10. FAQ: Foundry Sand Sieve Analysis

What is a good GFN for green sand casting?

There is no universal value. Light alloys and fine-detail work favor higher GFN (finer sand); heavy iron and steel sections favor lower GFN for permeability. GFN in the 45–60 range is common for green-sand iron work, but the distribution and fines content matter as much as the number itself.

How often should a foundry run a sieve analysis?

At minimum once per incoming sand lot, plus a routine weekly check on system sand where reclamation is active. High-volume iron foundries often run three per week, as in the cost model above, because drift can appear within days.

Does a higher GFN mean stronger mold sand?

Not directly. Higher GFN means finer grains, which raises surface area and bond demand and can raise green strength — but it lowers permeability. Strength, permeability and finish are competing goals; the right answer is a narrow distribution at the fineness your part requires.

Can two sands have the same GFN but perform differently?

Yes — that is the central finding of Section 5. A narrow sand and a bimodal sand can both report GFN 53 while differing threefold in fines and nearly threefold in permeability. Always specify the full distribution.

What is the difference between sieve analysis and a GFN?

Sieve analysis is the test and its output — the full particle-size distribution. The GFN is one summary number derived from that distribution. The test tells you more than the number does.

Ищете надежный металлургический завод в Китае?

  • Мы поможем вам оптимизировать конструкцию изделия и сократить расходы.
  • Мы можем помочь вам с изготовлением высококачественных литых деталей в больших объемах.
  • Мы можем осуществить поставку вовремя и получить больше возможностей на рынке сбыта.
  • Вы сможете воспользоваться услугами компании Supro MFG по литью металлов.

*Method per AFS 1106-00-S; sieves per ASTM E11. Cost figures are illustrative models, not supplier quotations. Data referenced from AFS publications, ASTM standards and Supro MFG shop-floor records.

Обеспечить наиболее экономически эффективное решение в области затрат на производство и сборку продукции, повышая конкурентоспособность продукции.

техническая команда, специализирующаяся на изготовлении корпусов на заказ уже более 30 лет.
Оборудование для высокотехнологичного производства: Ведущий в отрасли производитель металлических корпусов на заказ, располагающий собственными цехами по обработке листового металла, литью под давлением, прецизионной механической обработке и нанесению покрытий.

ISO 9001:2015, PPAP III уровня, RoHS, NEMA, CE и другие сертифицированные производственные стандарты.
Круглосуточная онлайн-поддержка на английском языке: команда профессионалов, говорящих по-английски, в любое время оперативно отвечает на технические вопросы пользователей в режиме онлайн.

оказывать пользователям помощь на всех этапах: от разработки продукта, создания прототипа, серийного производства, обработки поверхностей, сборки и упаковки до транспортировки, а также предоставлять ряд дополнительных услуг.

Благодаря наличию собственных механических и химических лабораторий компания может оперативно контролировать качество производственного процесса, что позволяет гарантировать поставку высококачественной продукции.

Согласиться подписать документы о неразглашении (NDA) для обеспечения защиты информации о продуктах клиентов.

Доставка «от двери до двери» в настраиваемой защитной упаковке с соблюдением условий доставки, согласованных с заказчиком.

Ищете надежного производителя?

Начать следующий проект в Supro MFG?

Прокрутить вверх