A casting defect claim is rarely lost in the metallurgy lab. It is lost in the first two days, when someone machines the suspect lot to keep the line running, throws away the sprue, and files the complaint three weeks later as an email that says “parts are bad, please advise.”
This article is written from the supplier side of that exchange, which is why it is unusually explicit: what evidence decides a claim, which defect signatures point to the drawing rather than the foundry, what a realistic recovery looks like on a 600-piece lot, and how to structure a settlement so the same argument does not repeat every quarter. The acceptance criteria referenced throughout come from published standards such as ASTM E446 for steel castings and ASTM A802 for surface acceptance, both of which name the severity levels a claim has to argue in.

Why Most Casting Defect Claims Collapse Before the Lab Report
In our own casting defect claim records, the majority of disputes that end in “no fault found” fail on process, not on metallurgy. Four failure modes account for almost all of them.
- The lot was consumed before it was frozen. Once a suspect casting is machined, the value at risk jumps from the casting price to the finished part price — on a machined pump housing that is roughly $42 of iron becoming $110 of finished part. The evidence (as-cast skin, gate location, sand adhesion) is also gone.
- No sample survived. A claim without a physical part is an opinion contest. Three pieces per defect mode, sealed and labelled with the pallet ID, is the minimum that lets a third party arbitrate.
- The drawing never said what “good” means. If the print shows only nominal dimensions, the supplier falls back on the default grade in ISO 8062-3, and a part that looks wrong to a buyer can be fully conforming on paper. That is a drawing problem, and no amount of inspection will fix it retroactively.
- The claim arrived after the window closed. Thirty days from receipt is the common contractual limit; sixty days is generous. A claim opened in month three is usually settled as a goodwill credit, not as a claim.
The practical rule we recommend to buyers is a 72-hour freeze: photograph the pallet before unpacking, quarantine the whole lot, keep the labels, and do not machine a single piece until the supplier has been notified in writing. It costs one shift of schedule. It is the difference between a recoverable casting defect claim and a discount request.
If the failure mode is still unclear at that point, the diagnostic order is fixed: visual and dimensional first, then non-destructive testing, then sectioning. The методы контроля литья article on this site walks through which method answers which question, and the Руководство по допускам при литье article covers the acceptance limits a claim has to quote.
What a Defensible Casting Defect Claim Contains
Nine documents decide a casting defect claim. Suppliers who receive all nine respond in days; suppliers who receive three respond with a request for more information, which is the polite form of a delay.
| Evidence item | What it decides | Who produces | Keep for |
|---|---|---|---|
| Pallet label, packing list, heat / lot number | Whether the parts are even from the batch under discussion | Buyer (photo) + supplier (traceability) | 24 months |
| Unpacking photos with a scale bar | Position of the defect on the part, and whether damage happened in transit | Buyer | Until closed |
| Non-conformance report with quantity and disposition | How many pieces, and what you want done (credit, sort, replace) | Buyer | 24 months |
| Dimensional report with datum scheme stated | Conformance to drawing versus conformance to standard | Buyer or supplier, CMM preferred | 24 months |
| Machining set-up sheet and program revision | Rules out fixture error and wrong-revision programs | Buyer | 12 months |
| Failed part, sectioned at the defect | Morphology: gas, shrinkage, inclusion, tear, or mechanical damage | Either side, jointly if possible | Until closed + 6 months |
| Third-party lab report (chemistry, metallography, SEM/EDS) | Independent attribution when the two sides disagree | Neutral lab, cost split by outcome | 5 years |
| Supplier process records: charge mix, pour temperature, sand test, mold hardness | Whether the process window was respected on that heat | Supplier | 12 months |
| Inspection certificate and delivery documents | What was actually certified, and under which standard (EN 10204 3.1 or 2.2) | Supplier | 5 years |
The 120-hour claim clock
A workable sequence for a casting defect claim that both sides can plan around, and that we use with our own accounts:
- Hour 0–4: quarantine, photograph, notify in writing with lot number and quantity.
- Hour 24: dimensional check and visual classification of every piece in the suspect lot; issue the non-conformance report.
- Hour 48: section two pieces at the defect; send one to the supplier, keep one sealed.
- Hour 72: supplier confirms receipt and states a position: contest, credit, or replace.
- Hour 120: if positions differ, agree a neutral lab and a cost-sharing rule in writing before the lab is instructed.
The single most expensive omission in that list is the sealed sample. Without it, the argument degenerates into comparing photographs taken under different lighting, which no arbitrator will resolve in your favour.

Casting Defect Liability: Reading the Failure Signature
Liability in a casting defect claim turns on origin, and origin is written into the morphology of the defect. The table below is the short version of how we triage a returned part, whether it came off a литье в песчаные формы line or an литье по выплавляемым моделям tree; the full defect catalogue with micrographs is in the common casting defects guide reference.
| Signature at the part | Most likely origin | Who normally carries the cost | First test |
|---|---|---|---|
| Straight crack at a section change, sharp internal corner | Design: fillet and section transition, not the pouring practice | Buyer / drawing owner | Dye penetrant + drawing check |
| Round gas pores clustered at the ingate or under the top surface, bright inner walls | Process: gating, mold permeability, gas in the melt | Supplier | Section + SEM |
| Irregular dark inclusions on the drag face, sand coloured | Process: sand system, core wash, mold closure | Supplier | Metallography |
| Spongy shrinkage at a heavy boss with no riser or chill | Shared: the riser design was agreed at DFM stage | Split, per the DFM record | Radiography, severity per ASTM E446 |
| Blowholes that appear only after 2.5 mm of machining allowance is removed | Process: gas entrapment below the skin | Supplier | Ultrasonic before machining |
| Dimensional drift inside the ISO 8062 default grade but outside the buyer’s expectation | Drawing: no tolerance class called out | Buyer | CMM + grade comparison |
| Chatter marks, wrong radius, or a bore 0.3 mm oversize after machining | Buyer: fixture, tool wear, program revision | Buyer | Set-up sheet + program log |
| Rust or staining on machined bores after a sea voyage | Shared: packaging and transit per Incoterm | Split, per delivery terms | Humidity indicator + VCI check |
The line between as-designed and as-supplied
The cleanest sentence in any quality agreement is this: the supplier is responsible for conformance to the drawing and to the standard named on it; the buyer is responsible for whether that drawing and that standard are adequate for the application. Everything else is negotiation.
That sentence resolves most disputes instantly. A 1.2 mm drift over a 480 mm span on a part whose drawing is silent about tolerance class is inside the ISO 8062-3 default grade for sand castings — the part conforms, and the claim is against the drawing. A hot tear at a 0.5 mm internal fillet is the same story: the foundry poured what was drawn. Conversely, gas porosity at the ingate is a process signature and stays with the supplier, no matter what the drawing says. The соглашение о качестве литья article sets out how to write those clauses so they survive a real argument.
Two further links in that chain are worth fixing before a claim happens: an agreed machining allowance (see the machining allowance article) determines whether a sub-skin defect is legitimately removed or exposed, and the первичный контроль продукции programme establishes the baseline a claim is measured against.
The Cost of a Casting Defect Claim: What Is Actually Recoverable
Here is a real-shaped example. A 600-piece lot of ductile iron pump housings from our чугунное литье line, casting price $42, machining value-add $68 at typical Обработка на станках с ЧПУ rates, arrives and passes sampling. During machining, 7.5% of the lot — 45 pieces — shows porosity at the flange face. The cost stack looks like this:
| Строка расходов | Расчет | Amount | Typical recovery |
|---|---|---|---|
| Casting value | 45 × $42 | $1,890 | Always |
| Machining value-add | 45 × $68 | $3,060 | Disputed; usually partial |
| Sorting the balance of the lot | 600 × $1.20 | $720 | Yes |
| Air freight for 300 replacement pieces | 1,440 kg × $2.70/kg | $3,888 | Yes if expedite was agreed |
| Engineering and admin time | 8 h × $65 | $520 | Rarely |
| Total exposure | — | $10,078 | — |
The supplier’s opening position will be $1,890, because that is the invoice value of the scrap. The gap is $8,188, and it is entirely made of costs the buyer incurred after the castings left the foundry. That gap is what a claim clause is for. Without a clause, the argument is settled by whoever has more schedule pressure.
Three settlement structures and their arithmetic
- Credit note only. Supplier credits $1,890 in castings; the buyer absorbs $8,188 of downstream cost. Fastest to close, worst economics, and it guarantees the next claim is argued the same way.
- Replacement lot plus sorting credit. Supplier casts and ships 45 replacements and credits the $720 sorting. The buyer re-machines 45 pieces at $3,060 and absorbs the schedule slip. Net buyer exposure roughly $3,060 plus lost capacity.
- Cost sharing on a 70/30 split. On a $10,078 stack, the supplier carries $7,055 and the buyer $3,023. This is the structure we see settle most often when cause is technically clear but the supplier’s process records are incomplete — and it is the structure that gets a corrective action agreed instead of an argument.
A default 50/50 split on unproven cause is the most expensive option available, because it teaches both sides that evidence does not pay. Over a two-year horizon the buyer usually ends up paying more per good piece through risk loading than the casting defect claim would ever recover. The total cost of ownership model is the right lens for that trade-off.

The sampling math that decides whether you can even see the defect
Incoming inspection is where most casting defect claims are either caught or created. Take a lot of 600 pieces, AQL 2.5, sample size 80, acceptance number 5 — a common ISO 2859-1 plan. At a 7.5% defect rate, the probability that this plan accepts the lot is 44%. In other words, more than four lots in ten would pass with 45 bad pieces inside.
Cost the two options against that: sampling costs 80 × $1.20 = $96 per lot, but carries an expected escape of 0.44 × 45 × $110 = $2,173, for about $2,269 per lot. Full inspection costs 600 × $1.20 = $720 and finds everything. Above roughly a 1% defect rate, 100% inspection is the cheaper plan; below it, sampling wins and the money is better spent on the supplier’s process control. That crossover is worth calculating once per part number instead of arguing about inspection philosophy every audit.
Four Controls That Stop the Next Casting Defect Claim
A casting defect claim closed is not a problem solved. These four controls, in this order, remove most of the recurrence risk, and each one is cheap compared with a single $10,078 event.
- 1. A frozen baseline. An approved first article with a signed dimensional report, a golden sample held by both sides, and a stated standard with its acceptance class. Everything later is measured against it rather than against memory. See the первичный контроль продукции procedure for the document set.
- 2. A change notification clause. Any change to pattern, gating, sand system, heat source or subcontractor requires written notice before the first affected shipment. Pattern work is where most of those changes originate, and the casting molds making process is the point at which they should be recorded.
- 3. A shared defect code list. Twelve codes agreed in writing — gas porosity, shrinkage, sand inclusion, hot tear, cold shut, misrun, dimension, surface, machining damage, packaging damage, chemistry, hardness — so that the first email already classifies the problem. It shortens the exchange by a week and makes trend data possible.
- 4. Retained samples and a 12-month data trail. Two pieces per lot kept by the supplier, photographs archived with the inspection record, and SPC on the two characteristics that matter. Without a trail, every casting defect claim starts from zero and ends in a split.
None of this substitutes for the supplier being able to run the process. The casting supplier audit checklist covers what to verify on site, and the литье в песчаные формы и литье по выплавляемым моделям comparison explains why the same defect vocabulary means different things in sand, investment and литье под давлением.
Where a claim does end in repair rather than replacement, the decision has its own arithmetic: the casting weld repair article sets out when welding or impregnation is legitimate and when it quietly transfers risk back to the buyer. Tied to the finishing steps in secondary operations, it also explains why some defects only become visible after shot blasting or passivation.
Frequently Asked Questions
Who pays for the machining cost on a defective casting?
Contractually, whoever accepted the risk of value-add. In practice, casting price plus a share of machining is the usual settlement when the defect was present as-cast and could not have been detected before machining without extra NDT. The supplier pays casting value only when the buyer machined a lot that had already been flagged, or skipped an agreed incoming inspection.
How long do I have to file a casting defect claim?
Thirty days from receipt is the common window, sixty is generous, and both are usually written into the quality agreement. Latent defects — those that appear only after machining or in service — are normally excluded from the clock but require proof that the cause existed at delivery. That proof is the retained sample and the lot number, which is why both should be contractual.
Can a foundry reject a claim because the parts were already machined?
It can, and often does, but not successfully if the evidence package holds. A machined part still carries the defect morphology: gas pores have round bright walls, shrinkage is dendritic and intergranular, inclusions have a mineral signature. What is genuinely lost is the ability to prove the part was not damaged after delivery, which is why the as-received photographs matter.
Do I need a third-party laboratory for a casting defect claim?
Only when the two sides disagree on origin, and then only one lab, jointly instructed, with the cost split agreed in writing before it starts. Chemistry plus metallography on a sectioned sample typically costs $300–$800 and settles questions that months of email cannot. Instructing two labs in parallel guarantees two reports that contradict each other and one more dispute.
What if the defect only appears after assembly or in service?
Then the claim becomes a failure investigation, and the burden shifts to showing the defect existed at delivery rather than being caused by assembly stress, over-torque or corrosion. Radiography of unmachined sister parts from the same heat, plus the supplier’s process records for that heat, is usually the deciding evidence. If neither exists, expect a goodwill credit rather than a recovery.
Does a simulation report help in a dispute?
Yes, when it was run before the tooling was cut and shows the riser and gating that were agreed. It converts “the foundry should have known” into a documented design decision, which is exactly what a shared-cause settlement needs. The casting simulation workflow describes what such a report has to contain to be usable later on.
Ищете надежный металлургический завод в Китае?
- Мы поможем вам оптимизировать конструкцию изделия и сократить расходы.
- Мы можем помочь вам с изготовлением высококачественных литых деталей в больших объемах.
- Мы можем осуществить поставку вовремя и получить больше возможностей на рынке сбыта.
- Вы сможете воспользоваться услугами компании Supro MFG по литью металлов.