Casting melt treatment is the short sequence of steps applied to metal between the furnace and the mold, and it decides whether the alloy on your drawing is the alloy you actually receive. Most buyers specify chemistry, tensile strength and X-ray class, then leave the molten-metal condition unwritten — which is exactly where hydrogen porosity, oxide films and unmodified eutectic silicon are decided.
This guide gives the numbers behind that window: hydrogen solubility ratios, density-index calculations, strontium and inoculant addition ranges, filtration selection, shop-floor release gates, and a worked payback model. Standards references are to ASTM E1251 for spark-AES chemistry, ASTM E155 for reference radiographs, and the 알루미늄 협회 for alloy and melt-handling practice. For the wider process context, start with our 금속 주조 가이드 and the casting inspection methods overview.

What Casting Melt Treatment Actually Controls
A heat can meet its chemistry specification and still produce scrap. Casting melt treatment targets three variables that a spectrometer alone does not see, and each one is locked in the moment the metal enters the cavity. Once poured, no amount of 열처리 or machining restores them.
- Dissolved gas. Hydrogen in aluminum alloys, hydrogen and nitrogen in steels. Solubility collapses during solidification, so the excess precipitates as micro-porosity that reduces fatigue life and pressure tightness — the mechanism explained in our porosity and shrinkage analysis.
- Non-metallic inclusions. Oxide films, dross particles, refractory fragments and bifilms entrained by turbulence. These act as crack initiators and are more damaging to fatigue than equivalent-size gas pores.
- Nucleation state. Eutectic silicon morphology in Al-Si alloys, graphite shape in irons, and as-cast grain size. Chemistry can be identical while elongation differs by a factor of two.
The practical constraint is time. In aluminum sand and 정밀 주조 the window from furnace tap to last pour is typically 8–15 minutes; for nodular iron it is 5–10 minutes before inoculation fades. That window is why casting melt treatment is a sequence with an order, not a list of optional additives: degas, then modify or inoculate, then filter, then pour and record.
| Variable | Shop-floor measure | Typical release criterion | If it is missed |
|---|---|---|---|
| Dissolved hydrogen | Reduced-pressure solidification sample, density index | DI ≤ 2.0% for structural A356 | Micro-porosity, failed radiograph, leak test rejects |
| Oxide / dross | Fracture sample, filter inspection, K-mold | No continuous film on fracture face | Fatigue failures, machined-surface tearing |
| Modification level | Thermal analysis cooling curve, eutectic undercooling ΔTE | ΔTE 8–12 °C for Sr-modified A356 | Coarse plate-like silicon, elongation loss |
| Inoculation / nodularity | Chill wedge, quick-cup microscopy | Nodularity ≥ 85%, chill depth ≤ 3 mm | Carbides, white iron edges, brittle castings |
| Chemistry | Spark-AES per ASTM E1251 | Within alloy limits before tap | Off-grade heat, wrong T6 response |
Note the last row. Casting melt treatment records are the only place these three variables appear together; chemistry is a gate, not a result: a heat inside specification can still carry 0.25 mL/100 g of hydrogen. Buyers who audit only the certificate are auditing the easiest 20% of the problem — a pattern that shows up repeatedly in scrap-rate investigations.
Degassing: Hydrogen, Density Index and the Reduced-Pressure Test
Hydrogen solubility in liquid aluminum near 700–750 °C is roughly 0.6–0.9 mL per 100 g, while the solid metal holds only about 0.03–0.05 mL per 100 g. That 15–20× drop is the whole reason gas porosity exists: the excess has to go somewhere, and it goes into interdendritic voids. Casting melt treatment removes it before the metal sees a mold.
In casting melt treatment, rotary degassing uses a graphite impeller at 300–550 rpm with argon or nitrogen at 6–15 L/min for 6–12 minutes per batch. Fine, inert bubbles sweep dissolved hydrogen out and float oxides to the dross layer. A one-tonne crucible commonly needs 8–10 minutes to reach a density index below 2%; doubling the gas flow does not halve that time, because the limit is bubble–metal contact area, not gas volume.
The reduced-pressure test solidifies a small sample under roughly 80–100 mbar alongside a sample solidified at atmospheric pressure. The density index is then: DI = (D_atm − D_vac) / D_atm × 100%. A worked example: D_atm = 2.682 g/cm³ and D_vac = 2.641 g/cm³ gives (0.041 / 2.682) × 100 = 1.53%, an acceptable structural melt. Drop D_vac to 2.605 and the same arithmetic gives 2.87%, which should be re-degassed rather than poured.
| Density index | Approx. hydrogen level | Typical application | Action |
|---|---|---|---|
| < 1.0% | Low, < 0.10 mL/100 g | Pressure-tight housings, aerospace-class radiography | Pour within 10 min |
| 1.0–2.0% | 0.10–0.15 mL/100 g | Structural A356-T6, hydraulic bodies | Normal release |
| 2.0–4.0% | 0.15–0.25 mL/100 g | Non-critical brackets, cosmetic parts | Re-degas if X-ray class is specified |
| > 4.0% | > 0.25 mL/100 g | None for quality castings | Hold the heat, find the moisture source |
Why a clean-looking surface still fails X-ray
Gas pores are internal and invisible on a ground surface, so visual inspection is not a release test. Reference radiographs such as ASTM E155 classify severity, but they only describe the result — they cannot tell you whether the cause was hydrogen, shrinkage or an oxide film. That distinction is why solidification simulation and a melt record have to be read together: a pore cluster in a hot spot is feeding, while uniformly distributed fine porosity across every section is gas.
Re-gassing is the underrated failure mode. A degassed bath held in humid air can climb from 1.5% to above 3% DI within 20–30 minutes, because moisture in the atmosphere and on damp tools reacts at the metal surface. The discipline that makes casting melt treatment work is therefore procedural: dry ladles, covered crucibles, and a hard rule that metal not poured within 10 minutes of the DI reading is re-tested. High-volume 다이캐스팅 cells automate this with inline degassing; jobbing 모래 주조 shops need the written rule instead.

Modification and Grain Refinement in Aluminum Castings
Unmodified A356 contains coarse, plate-like eutectic silicon. In the T6 condition that microstructure typically delivers 3–5% elongation; with proper strontium modification the silicon becomes fibrous and the same alloy reaches 8–12%. Casting melt treatment changes ductility without changing the chemistry certificate, which is why a buyer who specifies only the alloy designation has not actually specified the property they need.
Strontium is added as an Al-Sr10 master alloy at 100–200 ppm target residual, with real-world recovery of 60–80%. It needs 15–30 minutes of dissolution and gentle stirring to homogenize, and it fades over 3–4 hours of holding. Push past roughly 300 ppm and the treatment becomes counterproductive: over-modification coarsens the eutectic again and increases micro-porosity, especially when hydrogen is not under control first. Sodium at 0.008–0.02% works faster but fades in 30–60 minutes and contaminates crucibles, so it has largely been displaced in production foundries.
Grain refinement is a separate objective, and both additions live inside casting melt treatment rather than the alloy specification. An Al-5Ti-1B addition targeting 0.10–0.15% Ti and about 0.02% B can reduce as-cast grain size from 400–800 µm to 100–200 µm, cutting hot tearing in constrained geometries and improving feeding in thin sections. It is not a substitute for modification: one controls grain size, the other controls eutectic morphology. Alloy choice still sets the ceiling — see the A356 versus A380 comparison and our material substitution analysis.
| Addition | Typical target | Effective window | Verification | Main risk |
|---|---|---|---|---|
| Al-Sr10 (modification) | 100–200 ppm Sr residual | 3–4 h holding | Thermal analysis ΔTE 8–12 °C | Over-modification > 300 ppm raises porosity |
| Na-based modifier | 0.008–0.02% Na | 30–60 min | Fracture / thermal analysis | Fast fade, tool contamination |
| Al-5Ti-1B (refiner) | 0.10–0.15% Ti, ~0.02% B | 2–4 h | Grain size on quick-cup sample | Settling of TiB₂ particles in long holds |
| Rotary degassing | DI ≤ 2.0% | Re-test after 10 min | Reduced-pressure density index | Re-gassing from humid air |
| Ceramic foam filter | 10–30 ppi, 15–25 mm | Single pour | Visual + ΔP across filter | Blockage if metal is cold |
Read the cooling curve, not just the chemistry
Thermal analysis is the cheapest inline verification of modification level. A small quick-cup sample produces a cooling curve whose eutectic arrest shifts: unmodified A356 shows almost no eutectic undercooling, while a well-modified melt shows ΔTE of 8–12 °C. Foundries that log ΔTE per ladle can catch a missed Sr addition before 200 kg of metal is poured, rather than discovering low elongation after T6 heat treatment 그리고 CNC 가공 have already added value to the batch.
This is also where a casting melt treatment record protects both sides commercially. If a buyer later files a defect claim, the ΔTE and DI logs tied to a heat number show whether the loss came from the melt or from downstream handling — a distinction that our quality agreement template treats as a defined evidence item.
Inoculation and Nodularizing for Iron Castings
In iron, casting melt treatment is about graphite. Nodularizing with magnesium converts graphite from flakes to spheroids; inoculation then provides the nuclei that decide how many spheroids form and whether carbides appear in thin edges. Both steps decay with time, so the clock starts the moment the treatment ladle is filled.
For ductile iron, base sulfur should be below about 0.02% before Mg treatment, with residual Mg held at 0.03–0.06%. Below 0.03% the graphite reverts to compacted or flake forms; above 0.06% the melt is prone to dross, carbide formation and shrinkage. A well-treated ASTM A536 65-45-12 heat targets nodularity ≥ 85% and a nodule count above roughly 100/mm² in a 25 mm section. The difference is mechanical: gray iron with type-A graphite runs 200–300 MPa tensile with near-zero elongation, while 65-45-12 reaches about 450 MPa with 12% elongation — see the gray iron versus ductile iron comparison.
| Practice | Addition rate | Effective window | Chill / carbide risk | Where it fits |
|---|---|---|---|---|
| Ladle inoculation (FeSi75) | 0.2–0.6% | 5–12 min | Rises steeply after 8 min | General sand castings |
| Stream inoculation | 0.05–0.15% | At pour only | 낮음 | Thin-section, high-nodularity parts |
| In-mold inoculation | 0.05–0.10% | At pour only | 최저 | Automated high-volume lines |
| Mg treatment (FeSiMg) | Residual Mg 0.03–0.06% | 8–12 min before fade | Excess Mg promotes carbides | All nodular irons |
| No treatment | — | — | White iron in thin edges | Only for non-structural counterweights |
The eight-minute rule on the shop floor
Inoculation fade is not gradual in a way that operators can eyeball. A chill wedge poured immediately after inoculation might show 2 mm of white iron; the same metal poured eight minutes later can show 6 mm and produce hard spots that destroy tool life in machining. The operational answer is late inoculation — stream or in-mold — plus a hard maximum ladle-to-pour interval written into the work instruction. For alloy and grade selection beyond ductile iron, see cast steel grades 그리고 high-chrome white iron.
Iron work also ties directly to the mold: a well-inoculated melt will still shrink if the riser and gating are wrong. Treat the riser design guidance 그리고 pattern and mold design notes as parallel inputs, and use iron casting solutions when specifying the production route rather than a single heat.

Inclusion Control: Filtration and Charge Cleanliness
Degassing removes gas; it does not remove oxide films already in the metal. Bifilms — folded surface oxide entrained during pouring or transfer — behave like pre-existing cracks, and they are the usual explanation when two heats with identical DI values produce very different fatigue results. Casting melt treatment handles inclusions through charge discipline, quiet transfer and filtration.
Ceramic foam filters at 10–30 ppi and 15–25 mm thickness are placed in the runner or pouring cup. They work by impingement and adhesion rather than simple sieving, so metal velocity matters more than nominal pore size: keep flow near 0.5–1.0 kg/s per 100 × 100 mm of filter area. Under those conditions, capture of inclusions above roughly 20 µm is commonly 70–90%. A filter that is too fine for the pour rate simply raises the head requirement and can freeze off the runner.
| Filter | Typical alloy / process | Part type | Relative pressure drop | Notes |
|---|---|---|---|---|
| 10 ppi, 20 mm | Iron and steel, sand casting | Heavy sections, high flow | 낮음 | Coarse dross capture; pair with a dross trap |
| 20 ppi, 20 mm | Aluminum sand and gravity die | Housings, manifolds | 중간 | Most common general-purpose choice |
| 30 ppi, 15 mm | Aluminum investment, thin walls | Precision, pressure-tight parts | 높음 | Needs adequate metallostatic head |
| No filter | Non-critical counterweights | Cosmetic / balance weights | 없음 | Only where radiographic class is unspecified |
Charge cleanliness is the cheaper half of casting melt treatment. Cap returns at 30–40% of the charge, degrease and dry them before charging, and avoid plunging damp tools into the bath. The 알루미늄 협회 publishes melt-handling and alloy practice that is a reasonable baseline for supplier audits. Where a supplier cannot produce filter and charge records, treat the incoming inspection plan as the fallback control rather than assuming the melt was clean.
Downstream, the distinction matters commercially. Weld repair can close a surface defect but cannot remove distributed oxide films — our weld repair guide 그리고 nonconformance disposition framework both draw that line. Specifying casting melt treatment upstream is cheaper than arguing about disposition after the parts have been machined.
Measuring Casting Melt Treatment Before You Pour
A treatment that is not measured is a claim, not a control. The minimum credible shop-floor package has four instruments: a spark-AES spectrometer for chemistry (sampled per ASTM E1251), a thermal-analysis quick-cup for modification or inoculation level, a reduced-pressure solidification unit for density index, and a documented filter / dross check. None of them is expensive relative to a scrapped batch.
| Check | Method | Frequency | Release criterion | Record |
|---|---|---|---|---|
| Chemistry | Spark-AES chill-cast disc | Every heat, before tap | Inside alloy limits | Heat sheet, 3–7 yr retention |
| Hydrogen / DI | Reduced-pressure sample | Every ladle or transfer crucible | DI ≤ agreed limit (often 2.0%) | Sample photo + value + time |
| Modification / inoculation | Thermal analysis cooling curve | Every ladle for critical parts | ΔTE 8–12 °C (Al) / chill ≤ 3 mm (Fe) | Curve file tied to heat number |
| Cleanliness | Fracture sample, filter inspection | Each pour setup | No continuous oxide film | Photo + filter ppi / lot |
| Temperature | Immersion thermocouple | Each ladle | Within the agreed pouring window | Value + timestamp |
| Final verification | Radiography per ASTM E155 where specified | Per sampling plan | Agreed severity level | Report linked to heat number |
Three gates, one heat number
In a mature casting melt treatment system, the release logic is binary: chemistry, DI and thermal analysis all pass before the ladle is released; one failure sends the metal back for re-treatment rather than into a mold. Every record carries the same heat number that appears on the casting batch, the first article inspection report and the certificate. That single linkage is what turns a pile of measurements into traceability — and it is what a buyer needs when a field failure happens 18 months later.
Tie the same data into the tolerances guide and the quality agreement: dimensional capability depends on consistent solidification behaviour, and inconsistent melt condition shows up as scatter in shrinkage allowance long before it shows up as outright scrap. If the supplier audits are upcoming, ask for the raw DI and ΔTE logs, not a summary certificate.
What Casting Melt Treatment Costs and Where It Pays Back
Buyers often resist paying for melt control because it is invisible in the unit price. The arithmetic is straightforward once the yield effect is written down. Worked case: 60,000 A356 sand castings per year at 4.2 kg net each, fully loaded cost USD 18.40 per poured casting, baseline scrap 6.0%. Adding rotary degassing, filtration and ladle-by-ladle DI / thermal-analysis checks brings scrap to 3.6%.
At 6.0% scrap, the foundry must pour 60,000 / 0.940 = 63,830 castings to ship 60,000. At 3.6%, it pours 60,000 / 0.964 = 62,240. The difference is 1,590 castings that no longer consume metal, melting energy, molding time and cleaning labour: 1,590 × USD 18.40 = USD 29,256 per year. The treatment package costs USD 11,800 per year (rotor and gas, filters, master alloy, quick-cup consumables, sampling labour), leaving USD 17,456 net and a payback of about 8.1 months.
| Measure | Annual cost (USD) | Scrap rate | Gross saving (USD/yr) | Net (USD/yr) | Payback |
|---|---|---|---|---|---|
| Baseline (no formal control) | 0 | 6.0% | — | — | — |
| Rotary degassing + DI checks | 4,200 | 4.6% | 16,560 | 12,360 | 4.1 months |
| Add ceramic foam filtration | 3,100 | 4.0% | 23,460 | 16,160 | 4.9 months |
| Add thermal analysis per ladle | 2,400 | 3.7% | 27,600 | 17,900 | 6.3 months |
| Full package above | 11,800 | 3.6% | 29,256 | 17,456 | 8.1 months |
| Same package, gray iron counterweights | 9,600 | 1.8% → 1.3% | 3,100 | −6,500 | Never |
Who keeps the yield gain
The last row is the useful counterexample: on a non-critical gray iron counterweight with no radiographic requirement, the same package loses money. Casting melt treatment should be specified where the consequence of failure is real — pressure tightness, fatigue loading, structural T6 properties — not applied as a blanket surcharge. The second question is contractual: if the foundry cuts scrap from 6% to 3.6%, does the unit price fall at the next review, or does the supplier keep the gain until the tooling is amortized? Write it into the price adjustment clause or the quality agreement; otherwise a repeat RFQ quietly resets the baseline. Our cost breakdown 그리고 price-per-kg analysis show where yield assumptions hide in a quote.
Casting melt treatment pays twice: there is a scheduling benefit too. Fewer rejected castings means fewer remake queues, which shows up as delivery reliability rather than price; the lead-time model treats yield as a capacity multiplier. Buyers who reserve prototype capacity or use 3D-printed patterns for a bridge build should carry the same melt specification into production, or the prototype properties will not reproduce.
Specifying Casting Melt Treatment in the RFQ and PO
If it is not written into the enquiry, it will not be quoted, and if it is not quoted it will not be done. A usable casting melt treatment specification has eight fields. Each one needs a number or a named method — “good foundry practice” is not an acceptance criterion.
| Field | What to write | Evidence to request |
|---|---|---|
| Alloy and charge | Alloy designation + max 30–40% returns, degreased and dried | Heat sheet, charge log |
| Degassing | Rotary Ar/N₂ degassing; DI ≤ 2.0% per ladle; re-test after 10 min | DI value, time, sample photo |
| Modification / inoculation | Sr 100–200 ppm residual (Al) or residual Mg 0.03–0.06% + late inoculation (Fe) | Thermal-analysis curve, chill wedge |
| Filtration | 20 ppi × 20 mm ceramic foam in runner, flow ≤ 1.0 kg/s per 100 × 100 mm | Filter lot + setup photo |
| Chemistry | Spark-AES per ASTM E1251, before tap | Signed heat certificate |
| Release gate | All three gates pass; failed ladle re-treated, never poured | Ladle release log |
| Traceability | Heat number on casting batch, FAI and certificate; records 3–7 yr | Traceability matrix |
| Verification | Radiographic class per ASTM E155 where applicable | Radiographic report |
- Avoid vague standards. Writing “per applicable ASTM standards” without a DI limit or acceptance level leaves the supplier free to define the test. Name the method and the number.
- Ask for raw logs. A summary certificate confirms that a test existed; raw DI and ΔTE logs confirm when it was taken relative to the pour.
- Link to disposition. Define upfront what happens when a heat is poured out of specification — see the nonconformance framework for the four disposition paths.
Match casting melt treatment stringency to the route. 모래 주조 of large structural housings justifies the full package; 정밀 주조 of small precision parts adds tight filtration and temperature control; 고압 다이캐스팅 needs inline degassing and a short hold time rather than ladle-by-ladle sampling. Tooling decisions mold making 그리고 tooling cost are separate from melt control, but both belong in the same RFQ data pack so the quoted yield assumption is visible.
자주 묻는 질문
Is casting melt treatment the same as heat treatment?
No. Melt treatment happens to liquid metal before pouring and controls gas, inclusions and nucleation. Heat treatment happens to the solid casting afterwards and controls precipitates, matrix phases and stress relief. T6 cannot remove hydrogen porosity; degassing cannot produce a T6 temper. Both are needed for structural aluminum parts.
Can vacuum impregnation fix hydrogen porosity?
It can seal connected pores enough to pass a leak test, but it does not restore fatigue strength or fix a coarse, unmodified microstructure. Vacuum impregnation is a salvage route, not a substitute for melt control, and most quality agreements exclude it as a default disposition.
What density index should I specify for a structural A356 casting?
DI ≤ 2.0% is a practical production limit for structural parts, with ≤ 1.0% for pressure-tight or radiographically critical housings. Set the limit together with the radiographic class; a very tight DI on a non-critical part buys nothing and raises the quote.
Does melt treatment change the quoted price per kg?
Usually by a small line item — consumables, sampling labour and yield allowance. The larger effect is on how many castings must be poured to ship the ordered quantity, which is why the price-per-kg comparison and the yield assumption should be quoted together.
How often should a foundry record melt treatment data?
Chemistry per heat; DI and thermal analysis per ladle for critical parts; filter and temperature checks per pour setup. Records should carry the heat number and be retained 3–7 years, matching the FAI and certificate retention.
Can I skip casting melt treatment for prototype castings?
Only if the prototype is purely for fit and form. If mechanical test data from the prototype will be used to approve production, skip it and you will qualify a different material. Keep the same specification through prototype casting and production, or re-qualify explicitly.
신뢰할 수 있는 중국 금속 주조 공장을 찾고 계십니까?
- 우리는 제품 디자인을 최적화하고 비용을 절감하는 데 도움을 드릴 수 있습니다.
- 당사는 고품질의 대량 주조 부품 생산을 도와드릴 수 있습니다.
- 우리는 정시 배송을 완료하고 더 많은 판매 시장 기회를 확보할 수 있습니다.
- Supro MFG의 금속 주조 서비스를 이용하시면 많은 이점을 누리실 수 있습니다.
*Data referenced from ASTM E1251 / E155, Aluminum Association publications and Supro MFG shop-floor records. Values are typical production ranges; confirm limits for your alloy, section thickness and acceptance class with your foundry.