Casting filters are the cheapest insurance in a gating system, yet they are specified by habit more often than by calculation. Pick the wrong pore count or face area and you either pay for a filter that does nothing, or you starve the mold and create the misrun you were trying to prevent. This guide gives the arithmetic a buyer needs to specify them with confidence.
We cover filter area ratios, pore-density (PPI) pressure loss, pouring-basin buffer volume, placement, and the scrap credit that decides whether the filter pays for itself. Numbers come from first-order flow calculation and published foundry practice; the sizing method is the same one used in gating system engineering und flow turbulence control. For the fundamentals, start with the metal casting guide.

What Casting Filters Actually Remove (and What They Cannot)
A ceramic foam filter is a refractory strainer with an open, interconnected pore structure. Metal passes through; non-metallic inclusions larger than the pore throat are trapped on the front face and within the depth of the filter. The benefit is not just cleanliness — the filter also breaks a falling stream into many small laminar channels, which reduces re-oxidation and air entrainment downstream. That second effect is why filters often improve surface finish and porosity even when the inclusion count was already acceptable.
Be clear about the limits. Casting filters do not degas metal, do not remove dissolved hydrogen, and do not correct a badly designed sprue or an undersized riser. They capture solid particles. Dissolved gas must be handled at melt treatment, and fill sequencing belongs to the gating design. Treat the filter as the last barrier, not the whole strategy.
- Slag and dross films. Fragments broken up by pouring turbulence are the main target; these drive Häufige Gussfehler on machined faces.
- Sand and core wash particles. Erosion from the sprue, runner, or core prints is captured before it reaches the cavity.
- Refractory and furnace debris. Ladle lining and crucible spall show up as hard spots that destroy tool life.
Independent metrology matters here: quantify inclusion level before and after rather than judging by eye. The NIST metrology program is a useful reference for measurement discipline, and alloy-specific cleanliness expectations are published by the Aluminum Association.
Sizing Casting Filters: Choke Area, Face Velocity and the 2–4× Rule
Start with flow rate, not with a catalog size. For an A356 gravity pour of 8 kg in 6 seconds at a melt density of 2,400 kg/m³, the volumetric flow is 8 ÷ 2,400 ÷ 6 = 5.56 × 10⁻⁴ m³/s, or 556 cm³/s. With a 0.5 m metallostatic head, theoretical exit velocity is √(2 × 9.81 × 0.5) = 3.13 m/s; applying a discharge coefficient of 0.60 gives an effective 1.88 m/s. The choke area is therefore 5.56 × 10⁻⁴ ÷ 1.88 = 296 mm². This is the same choke calculation used in casting simulation workflows.
Filter face area should exceed choke area — commonly 2–4× — so the filter does not become the new choke. At a 3× ratio the face area is 887 mm², roughly a 30 × 30 mm effective window; face velocity falls to 0.63 m/s. At 4× it is 1,183 mm² and 0.47 m/s. The table shows the full set.
| Filter / choke area ratio | Face area (mm²) | Equivalent square side (mm) | Face velocity (m/s) |
|---|---|---|---|
| 1× (filter = choke) | 296 | 17.2 | 1.88 — filter now controls fill |
| 2× | 591 | 24.3 | 0.94 |
| 3× | 887 | 29.8 | 0.63 |
| 4× | 1,183 | 34.4 | 0.47 |
A filter is rated by gross face dimension, but the frame and seating land consume part of it. Specify the effective opening, and confirm the supplier’s frame is included in the quoted size. For high-volume programs this detail is usually written into the quality agreement; for one-off work it belongs in the RFQ.
Why face velocity matters more than nominal size
If face velocity is too high, the filter adds head loss and can freeze off early; if too low, there is little flow to push inclusions into the pore structure and the filter works only as a coarse screen. A practical aluminum window is roughly 0.2–0.6 m/s face velocity. In our example, a 2× ratio (0.94 m/s) is already outside that window — which is why “one size smaller to save money” is a false economy.
Choosing Casting Filters by PPI: The Head-Loss Trade-Off
Pores per inch (PPI) sets the capture threshold and the resistance. Finer filter media trap smaller inclusions but cost more head. A first-order Darcy estimate makes the trade visible. For aluminum at 1,300 °C, take dynamic viscosity μ = 0.0013 Pa·s, filter thickness L = 50 mm, density 2,400 kg/m³, and engineering permeabilities of 1.5 × 10⁻⁸ m² (10 PPI), 5 × 10⁻⁹ m² (20 PPI) and 2 × 10⁻⁹ m² (30 PPI). Pressure drop is ΔP = μ · v · L / k, and metal head loss is ΔP ÷ (ρg).
At a 0.22 m/s face velocity: 10 PPI loses about 40 mm of metal head, 20 PPI about 121 mm, and 30 PPI about 304 mm. The last figure exceeds the 300 mm of head in many gravity layouts — the mold can stop filling before the cavity is full. This is the single most common specification error we see, and it explains why a “better” filter can produce a worse casting.
| PPI | Head loss @ 0.15 m/s | @ 0.22 m/s | @ 0.35 m/s | Typical use |
|---|---|---|---|---|
| 10 | 28 mm | 40 mm | 64 mm | Coarse iron, large runners |
| 20 | 83 mm | 121 mm | 193 mm | General aluminum and iron work |
| 30 | 207 mm | 304 mm | 483 mm | Critical cosmetic faces, tall head |
These are first-order estimates: inertial losses at higher velocity add to the Darcy term, so measured drop will be somewhat larger. Use them to rank options, then confirm with a fill trial. The same head budget logic applies to pouring temperature — extra head loss costs superheat, and superheat costs energy and gas pickup.

Pouring Cups and Basins: Feeding Casting Filters Without a Vortex
The pouring cup is part of the filter system whether you count it or not. Its job is to keep the sprue full, damp the falling stream, and buffer the operator’s inevitable pause. A simple cup is not enough: at our 556 cm³/s flow rate, a 90 × 70 × 45 mm cup holds only 284 cm³ — about 0.51 seconds of buffer. One second of hesitation uncovers the sprue, air is drawn in, and the filter is fed a two-phase stream.
A stepped basin of 120 × 90 × 60 mm holds 648 cm³ (1.17 s); a 150 × 110 × 70 mm basin holds 1,155 cm³ (2.08 s). That is why production cells use basins, not cups, whenever the pour is operator-controlled. Offset the sprue well and add a dam or a ceramic filter at the cup exit so dross floats instead of being sucked down — the same principle used in green sand und energy-efficient melting practice.
| Cup / basin | Volume (cm³) | Buffer at 556 cm³/s | Verdict |
|---|---|---|---|
| Cup 90 × 70 × 45 mm | 284 | 0.51 s | Too small for manual pour |
| Basin 120 × 90 × 60 mm | 648 | 1.17 s | Acceptable, steady operator |
| Basin 150 × 110 × 70 mm | 1,155 | 2.08 s | Preferred for critical work |
Casting Filters in the Runner vs the Sprue: Placement That Works
Place the filter as close to the casting as practical, but after the dross-collecting features. In a horizontal runner, the filter should sit flat with a machined or well-compacted seat; any gap along the edge lets unfiltered metal bypass it. In a vertical sprue, gravity holds the filter in place but thermal shock is harsher — preheat or pour through promptly. For Sandguss programs we favor horizontal runner seating; for Feinguss shells, a cup-filter combination is usual.
Four placement rules
- Seat area is part of the filter. Order by effective opening, not the outer frame.
- Support both faces. A filter that deflects under head cracks and becomes a new inclusion source.
- Keep the runner full downstream. A partially filled runner after the filter reintroduces air; see porosity control.
- One filter per sprue, sized once. Stacking filters to “increase filtration” multiplies head loss — the opposite of what is wanted.
For high-pressure work, Druckguss uses different filtration hardware because fill times are far shorter; do not transfer sand-mold PPI rules directly. Our degating und riser sleeve guides cover what happens downstream of the filter.
What Casting Filters Cost — and the Scrap Credit That Pays for Them
Take an A356 program of 12,000 parts per year, 8 kg each, with a $0.62 filter. Annual filter cost is 12,000 × $0.62 = $7,440. If inclusion-driven scrap falls from 4.0% to 1.2%, that recovers 12,000 × 0.028 = 336 parts.
Here is the part that changes the decision. Each recovered casting carries $18 of metal and $24 of downstream CNC-Bearbeitung value — $42 total. Full scrap credit is 336 × $42 = $14,112/year, so the net gain is $6,672 and the return is 1.90× on filter spend. But if you credit only the metal value, 336 × $18 = $6,048 — $1,392 less than the filter cost. The filter looks like a loss. Same casting, same filter, opposite answer, depending on whether machining is counted.
| Credit basis | Recovered value / yr | Net vs $7,440 filter cost |
|---|---|---|
| Metal only ($18/part) | $6,048 | −$1,392 (false loss) |
| Metal + machining ($42/part) | $14,112 | +$6,672 (1.90×) |
Break-even scrap reduction
How much scrap drop do you actually need? Divide annual filter cost by annual volume and recovered value per part. At $0.45 per filter the break-even is 1.07 percentage points; at $0.62 it is 1.48 pp; at $0.95 it is 2.26 pp. If your measured inclusion scrap is below 1%, a fine filter probably cannot pay for itself on scrap credit alone — justify it on claim avoidance or customer mandate instead. Cost-of-quality framing is explored in our price-per-kg analysis.

30-Day Trial Plan and RFQ Checklist for Casting Filters
Do not switch filters across a whole program at once. Run a controlled trial: Week 1 — baseline inclusion scrap by part number. Week 2 — install one filter size at 3× choke ratio, log fill completeness and head loss symptoms. Week 3 — vary PPI only, holding face area constant. Week 4 — confirm with a machined-face inspection and lock the specification. For tooling and fixture context, see molds making and our prototype casting service.
- Alloy and pour weight. Sets density, viscosity and required flow rate.
- Pour time and metallostatic head. Needed to compute choke area and available head loss.
- Effective face area and frame size. State both; ask for the seating-land allowance.
- PPI and filter thickness. Head loss scales with both.
- Placement sketch. Runner or sprue, upstream dross trap, downstream runner length.
- Acceptance criterion. Inclusion count per machined face, or scrap percentage by cause.
Buyers building a supply package often combine this with iron casting or Aluminiumguss capability review and a casting alloy selection check, since alloy choice changes both viscosity and inclusion morphology. Process safety in the pouring area should follow NFPA guidance; welding and repair of fixtures follows AWS practice. Ask us for a filter trial on your next RFQ.
Validating Casting Filters: Sectioning, Radiography and Machined-Face Inspection
A filter is only proven if you measure the result. The weakest evidence is a visual check of the as-cast surface — most inclusions that matter are buried below the skin and only appear after the first machining pass. Stronger evidence comes from a section through the runner and the casting. Cut the trial mold along the gating plane, polish the section, and look at the upstream face of the filter. A loaded filter should show a dark cake of slag and sand particles; a clean face after a dirty pour means metal bypassed the media through a gap in the seat. That single observation tells you more than a week of scrap statistics.
Radiography is the second line of evidence for internal defects. It is slow and costs money per part, so use it on the first articles of a trial rather than on production. Compare a baseline part cast without casting filters against a filtered part at the same pour temperature and head. If the radiographs look identical, the filter is not earning its place — either the melt was already clean or the wrong PPI was chosen. For high-value components, pair radiography with a machined-face inspection at the exact surface the customer will finish; that is where inclusion-related rework is booked.
Choosing a validation method
Match the method to the failure mode. A customer rejecting cosmetic faces needs surface inspection; a parts failing pressure test needs radiography or sectioning. Record the inclusion count by cause, not just the total scrap percentage — a drop in sand inclusions with no change in gas porosity is exactly what casting filters should deliver, and it prevents the wrong conclusion about what the filter can do.
| Method | What it proves | Best used for |
|---|---|---|
| Runner sectioning | Filter loaded, no bypass channel | First trial mold, seat verification |
| Radiography | Internal inclusion and shrinkage level | Pressure-tested and critical parts |
| Machined-face count | Customer-visible defect frequency | Scrap credit calculation |
Keep the samples. A photographed cross-section of a loaded filter is the most persuasive artifact in a quality agreement conversation, because it converts an abstract claim about cleanliness into physical evidence both engineers can see.
How long does a filter last in production
In jobbing sand work, casting filters are normally single-use: one filter per mold, discarded after shakeout. The relevant question is not lifespan but loading rate. If the front face becomes fully blocked before the cavity fills, the media was undersized or the melt was far dirtier than assumed — the symptom is a short pour or a cold shut at the last section to fill. Track the number of pours per filter in any semi-continuous setup, and set a replacement trigger based on measured head loss rather than elapsed time. A filter that still passes flow but has a fully loaded face is no longer removing inclusions; it has become an expensive piece of refractory in the runner. Conversely, a filter that comes out clean after a dirty heat is a sign of bypass, not of a clean melt. Simple weigh-before and weigh-after checks on a sample of used casting filters will tell you which regime you are in, and that record is far more useful than a supplier’s nominal loading-capacity figure.
Casting Filters by Alloy: Adjusting PPI and Head Budget
The head-loss table above was built for aluminum. Other alloys change viscosity, density and the inclusion morphology the casting filters must catch. Ductile iron at roughly 1,450 °C has a higher density, so the same pressure drop consumes less metallostatic head in millimetres; against that, iron pours are often dirtier and need a coarser media to avoid rapid loading. A 10–20 PPI window is common for iron, while aluminum work usually sits at 20 PPI and critical faces at 30 PPI. Steel needs refractory grades rated for the higher pouring temperature and a seating system that survives the thermal shock.
Do not convert between alloys by holding the same filter part number. Recompute flow from pour weight and density, recompute choke area from head, then choose PPI from the alloy’s inclusion requirement and recheck the head budget. A filter that worked in an A356 program can starve a gray-iron casting with a different runner layout — not because the media changed, but because the flow and head did. Alloy, geometry and filter specification are one calculation, not three independent choices. This is why a supplier asking only for the alloy name cannot size casting filters correctly.
| Alloy family | Typical PPI window | Main constraint |
|---|---|---|
| Aluminum (A356, A380) | 20–30 | Head loss vs cosmetic finish |
| Grauguss und duktiles Gusseisen | 10–20 | Loading rate from dirty melts |
| Cast steel | 10–20, high-temperature grade | Refractory rating and thermal shock |
Häufig gestellte Fragen
Do casting filters remove gas porosity?
No. They trap solid inclusions and laminarize flow, which indirectly reduces air entrainment. Dissolved hydrogen requires degassing or melt treatment before pouring.
Is a higher PPI always better?
No. In the worked example, 30 PPI consumed about 304 mm of metal head at 0.22 m/s — enough to stop fill in a typical gravity mold. Choose the coarsest PPI that meets the inclusion requirement.
How do I know the filter is not being bypassed?
Section a trial casting through the runner. Metal should show a clean upstream face on the filter with no unfiltered stream along the seat edge; a gap leaves a bright channel around the frame.
Can one filter serve several cavities?
Yes, if the filter is sized from the total choke area of the combined gating system, not from a single cavity. Undersizing is a common cause of unbalanced fill in multi-cavity molds.
When is filtration not worth the cost?
When measured inclusion scrap is already below roughly 1% and the part has little downstream machining value. In that case the break-even scrap drop exceeds what filtration can deliver.
Suchen Sie eine zuverlässige Metallgießerei in China?
- Wir können Ihnen dabei helfen, das Produktdesign zu optimieren und Kosten zu sparen.
- Wir können Ihnen bei hochwertigen Gussteilen in großen Stückzahlen helfen.
- Wir können pünktlich liefern und uns mehr Absatzmarktchancen erschließen.
- Sie werden vom Metallguss-Service von Supro MFG profitieren.
*Data referenced from published foundry practice, NIST / Aluminum Association / DOE IEDO guidance and Supro MFG shop-floor records. Head-loss figures are first-order Darcy estimates for option ranking; confirm by fill trial.