{"id":8188,"date":"2026-11-02T01:30:41","date_gmt":"2026-11-02T01:30:41","guid":{"rendered":"https:\/\/chinametalfoundry.com\/?p=8188"},"modified":"2026-11-03T04:15:02","modified_gmt":"2026-11-03T04:15:02","slug":"high-chrome-white-iron-castings","status":"publish","type":"post","link":"https:\/\/chinametalfoundry.com\/ru\/blog\/high-chrome-white-iron-castings\/","title":{"rendered":"\u041e\u0442\u043b\u0438\u0432\u043a\u0438 \u0438\u0437 \u0431\u0435\u043b\u043e\u0433\u043e \u0447\u0443\u0433\u0443\u043d\u0430 \u0441 \u0432\u044b\u0441\u043e\u043a\u0438\u043c \u0441\u043e\u0434\u0435\u0440\u0436\u0430\u043d\u0438\u0435\u043c \u0445\u0440\u043e\u043c\u0430: \u043c\u0430\u0440\u043a\u0438 A532, \u0432\u0438\u0434\u044b \u0438\u0437\u043d\u043e\u0441\u0430 \u0438 \u0441\u0442\u043e\u0438\u043c\u043e\u0441\u0442\u044c \u0432 \u0447\u0430\u0441"},"content":{"rendered":"<article class=\"sc-article\" style=\"max-width: 820px; margin: 0 auto; font-family: 'Poppins',sans-serif; color: #7e7e7e; font-size: 16px; line-height: 1.7;\">\n<div class=\"sc-intro\" style=\"background: #F5F5F5; border-radius: 20px; padding: 22px 24px; font-style: italic; color: #3a3a3a; margin: 0 0 26px; line-height: 1.6;\">\n<p style=\"margin: 0;\"><strong style=\"color: #273171;\">High chrome white iron castings<\/strong> are bought for one reason: the part has to survive abrasive wear that eats mild steel in a matter of weeks. Every other number in the quotation \u2014 price per kilogram, lead time, surface finish \u2014 is secondary to whether the carbide structure inside the metal matches the way the part actually wears. This guide is about that decision, in numbers.<\/p>\n<\/div>\n<p style=\"margin: 0 0 18px;\">What follows is the working view from a foundry floor: what an abrasion-resistant iron is under <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/www.astm.org\/a0532_a0532m-10.html\" target=\"_blank\" rel=\"noopener\">ASTM A532\/A532M<\/a>, how carbon and chromium set the carbide volume fraction, where the four wear modes break these parts, and two cost-per-operating-hour models that show when the premium alloy pays for itself and when it does not. Hardness conditions and chemistry limits are quoted from the standard rather than from a marketing sheet. Suppliers of the finished parts, and buyers checking them, can cross-reference the material data with <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/www.nadca.com\/\" target=\"_blank\" rel=\"noopener\">NADCA<\/a> on casting quality and the <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/ru\/%d0%b1%d0%bb%d0%be%d0%b3\/%d1%80%d1%83%d0%ba%d0%be%d0%b2%d0%be%d0%b4%d1%81%d1%82%d0%b2%d0%be-%d0%bf%d0%be-%d0%bb%d0%b8%d1%82%d1%8c%d1%8e-%d0%bc%d0%b5%d1%82%d0%b0%d0%bb%d0%bb%d0%be%d0%b2\/\" target=\"_blank\" rel=\"noopener\">\u0440\u0443\u043a\u043e\u0432\u043e\u0434\u0441\u0442\u0432\u043e \u043f\u043e \u043b\u0438\u0442\u044c\u044e \u043c\u0435\u0442\u0430\u043b\u043b\u043e\u0432<\/a> on the base process.<\/p>\n<h2 style=\"font-family: 'Poppins',sans-serif; color: #273171; font-size: 25px; font-weight: 600; line-height: 1.3; margin: 34px 0 14px; padding: 4px 0 4px 30px; background: linear-gradient(to right, #ff512f 0px, #dd2476 5px, transparent 5px);\">What High Chrome White Iron Castings Are \u2014 and What They Are Not<\/h2>\n<p style=\"margin: 0 0 18px;\">A white cast iron is an iron that solidifies without graphite. All the carbon is tied up in carbides, which is exactly what makes the material wear-resistant and exactly what makes it brittle. ASTM A532 covers the alloyed branch of that family: irons alloyed to secure high resistance to abrasive wear for mining, milling, earth-handling and general manufacturing duty. The standard explicitly excludes plain and low-alloy white irons that consist of iron carbides in a pearlite matrix \u2014 those are hard but not tough enough to be sold as wear parts. The casting route itself is ordinary iron foundry work, <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/ru\/%d0%bb%d0%b8%d1%82%d1%8c%d0%b5-%d0%b2-%d0%bf%d0%b5%d1%81%d1%87%d0%b0%d0%bd%d1%8b%d0%b5-%d1%84%d0%be%d1%80%d0%bc%d1%8b\/\" target=\"_blank\" rel=\"noopener\">\u043b\u0438\u0442\u044c\u0435 \u0432 \u043f\u0435\u0441\u0447\u0430\u043d\u044b\u0435 \u0444\u043e\u0440\u043c\u044b<\/a> or shell moulding, with gating, pouring temperature and shakeout time doing the metallurgy rather than the moulding method.<\/p>\n<p style=\"margin: 0 0 18px;\">Inside an A532 casting the microstructure is carbides in a matrix of martensite, bainite or austenite. That combination is the whole design: the carbides resist the abrasive particle, the matrix holds them in place and absorbs the load that would otherwise crack the part. Get the matrix too soft and the carbides spall out of it; get the matrix too hard and the whole casting behaves like glass. This is a different mechanism from the graphitic irons, where flake or nodular graphite controls strength and damping rather than wear, as set out in our comparison of <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/ru\/%d0%b1%d0%bb%d0%be%d0%b3\/%d1%81%d0%b5%d1%80%d1%8b%d0%b9-%d1%87%d1%83%d0%b3%d1%83%d0%bd-%d0%b8-%d0%b2%d1%8b%d1%81%d0%be%d0%ba%d0%be%d0%bf%d1%80%d0%be%d1%87%d0%bd%d1%8b%d0%b9-%d1%87%d1%83%d0%b3%d1%83%d0%bd\/\" target=\"_blank\" rel=\"noopener\">gray iron versus ductile iron<\/a> and our breakdown of <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/ru\/%d0%b1%d0%bb%d0%be%d0%b3\/cast-iron-vs-cast-steel\/\" target=\"_blank\" rel=\"noopener\">cast iron versus cast steel<\/a>.<\/p>\n<p style=\"margin: 0 0 18px;\">The practical consequence for a buyer is that high chrome white iron castings cannot be judged on a tensile test. A 26% Cr iron will show a transverse rupture strength in the region of 900\u2013950 MPa and a compressive strength near 2,900 MPa, but essentially no elongation. The material is being asked to resist indentation and scratching, not to stretch. That is why the acceptance test that matters is hardness, measured in a defined place, on a defined test block.<\/p>\n<table style=\"width: 100%; border-collapse: collapse; margin: 18px 0 24px; font-size: 15px; color: #333333;\">\n<thead>\n<tr>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Family<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Typical hardness<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Carbon form<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Impact tolerance<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Weld repair<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Typical duty<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Gray iron (ASTM A48)<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">170\u2013250 HB<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Flake graphite<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Low, but predictable<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Difficult<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Housings, bases, damped structures<\/td>\n<\/tr>\n<tr style=\"background: #F5F5F5;\">\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Ductile iron (ASTM A536)<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">150\u2013300 HB<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Nodular graphite<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Good, 6\u201318% elongation<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Possible with procedure<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Brackets, pump bodies, gears<\/td>\n<\/tr>\n<tr>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">High chrome white iron (A532 Cl. III)<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">450\u2013700 HB<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">M<sub>7<\/sub>C<sub>3<\/sub> carbides<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Very low<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Not permitted<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Slurry pumps, chute liners, mill internals<\/td>\n<\/tr>\n<tr style=\"background: #F5F5F5;\">\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Hadfield manganese steel (A128)<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">200 HB as cast, work-hardens to 450\u2013500 HB<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Austenitic, no carbide network<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Very high<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Possible with procedure<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Jaw plates, gyratory concaves, hammer mills<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<h2 style=\"font-family: 'Poppins',sans-serif; color: #273171; font-size: 25px; font-weight: 600; line-height: 1.3; margin: 34px 0 14px; padding: 4px 0 4px 30px; background: linear-gradient(to right, #ff512f 0px, #dd2476 5px, transparent 5px);\">The Carbide Structure That Makes White Iron Wear Resistant<\/h2>\n<p style=\"margin: 0 0 18px;\">Two carbides matter. Cementite, M<sub>3<\/sub>C, carries roughly 6.7% carbon by weight and sits at about 900\u20131,100 HV. The chromium carbide M<sub>7<\/sub>C<sub>3<\/sub> carries 8.44% carbon and sits at roughly 1,200\u20131,800 HV, and it grows as isolated rods and blades rather than as a continuous network. That shape difference is why high chrome white iron castings survive a silica particle that a low-alloy white iron cannot: the abrasive has to cut through discrete hard islands instead of following a connected brittle skeleton that cracks through the casting.<\/p>\n<p style=\"margin: 0 0 18px;\">For high chrome white iron castings the variable a foundry controls to choose between them is not chromium percentage alone, it is the chromium-to-carbon ratio. Once that ratio passes about 5, M<sub>7<\/sub>C<sub>3<\/sub> dominates; below about 4.5, a substantial share of the carbon reports as cementite and the wear resistance drops even though the hardness figure can look respectable.<\/p>\n<ul style=\"margin: 0 0 18px; padding-left: 22px;\">\n<li style=\"margin: 0 0 8px;\"><strong style=\"color: #273171;\">26.5% Cr with 2.50% C<\/strong> \u2014 ratio 10.6, fully M<sub>7<\/sub>C<sub>3<\/sub>. The standard 25\u201327% Cr pump and liner grade.<\/li>\n<li style=\"margin: 0 0 8px;\"><strong style=\"color: #273171;\">26.5% Cr with 3.40% C<\/strong> \u2014 ratio 7.8, hypereutectic. Primary carbide blades form in the melt, wear resistance peaks, toughness falls.<\/li>\n<li style=\"margin: 0 0 8px;\"><strong style=\"color: #273171;\">15% Cr with 3.00% C<\/strong> \u2014 ratio 5.0, borderline. Cheaper, adequate for moderate abrasion, noticeably more brittle in thin sections.<\/li>\n<li style=\"margin: 0 0 8px;\"><strong style=\"color: #273171;\">12% Cr with 3.00% C<\/strong> \u2014 ratio 4.0, mixed carbide. Sold as a wear iron, behaves like a hardened alloy steel with carbide reinforcement.<\/li>\n<\/ul>\n<p style=\"margin: 0 0 18px;\">Carbon also sets how much carbide there is, and this is arithmetic a buyer can check. Taking the matrix as retaining about 0.6% C in solution and M<sub>7<\/sub>C<sub>3<\/sub> as 8.44% C, a 2.50% C iron puts 1.90% C into carbide, which is 22.5% carbide by mass. Correcting for the density difference between carbide (about 6.9 g\/cm\u00b3) and matrix (about 7.7 g\/cm\u00b3) gives roughly 24.5% carbide by volume. Raise carbon to 3.40% and the same arithmetic gives 33.2% by mass and about 36% by volume.<\/p>\n<table style=\"width: 100%; border-collapse: collapse; margin: 18px 0 24px; font-size: 15px; color: #333333;\">\n<thead>\n<tr>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Carbon<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Cr:C at 26.5% Cr<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Carbide by volume<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Wear resistance<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">What it costs you<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">2.50%<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">10.6<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">\u224824.5%<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Reference<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Baseline toughness, easiest to cast and harden<\/td>\n<\/tr>\n<tr style=\"background: #F5F5F5;\">\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">2.90%<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">9.1<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">\u224829%<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">+15\u201325% in low-stress sliding<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Higher pouring temperature needed, more shrinkage<\/td>\n<\/tr>\n<tr>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">3.40%<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">7.8<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">\u224836%<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">+35\u201350%, best in fine-particle slurry<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Hypereutectic carbides settle, thin sections crack<\/td>\n<\/tr>\n<tr style=\"background: #F5F5F5;\">\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">3.60%+<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">7.4<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">\u224840%<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Maximum abrasion resistance<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Machining almost impossible, impact tolerance near zero<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p style=\"margin: 0 0 18px;\">The number that decides whether you get the carbide you paid for is the cooling rate. Slow cooling in a heavy sand section lets chromium partition and lets the carbide network coarsen; fast cooling in a thin section chills the iron and can crack it before it reaches the shakeout. That is why the same certified chemistry can deliver 640 HB on a 40 mm wear block and 520 HB in the 180 mm hub of a pump casing, and why the hardness clause on a purchase order has to name the location of the test.<\/p>\n<figure style=\"margin: 24px 0;\"><img decoding=\"async\" style=\"width: 100%; display: block; border-radius: 4px;\" src=\"https:\/\/chinametalfoundry.com\/wp-content\/uploads\/2026\/11\/p252-hcwi-cover.webp\" alt=\"High chrome white iron castings for slurry pump duty, impeller and pump casing on a foundry bench\" \/><figcaption style=\"font-size: 13px; color: #7e7e7e; text-align: center; margin-top: 8px;\">High chrome white iron castings for slurry duty: the impeller and casing are the two parts where carbide volume fraction decides maintenance cost.<\/figcaption><\/figure>\n<h2 style=\"font-family: 'Poppins',sans-serif; color: #273171; font-size: 25px; font-weight: 600; line-height: 1.3; margin: 34px 0 14px; padding: 4px 0 4px 30px; background: linear-gradient(to right, #ff512f 0px, #dd2476 5px, transparent 5px);\">Reading the ASTM A532 Grade Table for High Chrome White Iron Castings<\/h2>\n<p style=\"margin: 0 0 18px;\">ASTM A532 organises high chrome white iron castings into three classes. Class I is the nickel-chromium family usually traded as Ni-Hard, with around 4% Ni and 2% Cr: cheap, well understood, decent in cement slurry, but well behind the high-chrome grades on both hardness and corrosion resistance. Class II is the low-carbon nickel-chromium variant, tougher and used where a casting has to take some shock. Class III is the high-chromium family, and Class III Type A is the grade that most high chrome white iron castings in the market actually are.<\/p>\n<p style=\"margin: 0 0 18px;\">The chemistry window for Class III Type A, as published in the standard and reproduced by pump OEMs in their own purchase specifications, is broad: carbon 2.0\u20133.3%, chromium 23\u201330%, manganese up to 2.0%, silicon up to 1.5%, molybdenum up to 3.0%, nickel up to 2.5%, copper up to 1.2%, phosphorus 0.10% max, sulphur 0.06% max. That width is deliberate \u2014 it lets a foundry tune carbon for the wear mode and add molybdenum and copper for section thickness. It also means two suppliers can both ship &#8220;A532 Class III Type A&#8221; and deliver parts with meaningfully different wear life.<\/p>\n<p style=\"margin: 0 0 18px;\">Hardness is specified by condition rather than as a single number, and this is where most quotation disputes start:<\/p>\n<table style=\"width: 100%; border-collapse: collapse; margin: 18px 0 24px; font-size: 15px; color: #333333;\">\n<thead>\n<tr>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Condition supplied<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Hardness requirement<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">What it is for<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">As cast<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">\u2265450 HB (\u226546 HRC, \u2265485 HV)<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Cheap wear plate, low impact, no machining after casting<\/td>\n<\/tr>\n<tr style=\"background: #F5F5F5;\">\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">As cast and stress relieved<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">\u2265450 HB<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Large castings that would otherwise crack in service from residual stress<\/td>\n<\/tr>\n<tr>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Hardened<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">\u2265600 HB (\u226556 HRC, \u2265660 HV)<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Pump internals, mill liners, anything with a real wear rate to beat<\/td>\n<\/tr>\n<tr style=\"background: #F5F5F5;\">\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Hardened and stress relieved<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">\u2265600 HB<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Hardened parts with a heavy section change or a machined fit<\/td>\n<\/tr>\n<tr>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Softened for machining<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">\u2264400 HB (\u226441 HRC, \u2264430 HV)<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">The route that lets you drill, tap and bore before final hardening<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p style=\"margin: 0 0 18px;\">The last row is the one engineers most often miss. Above roughly 500 HB you can grind and face a high-chrome part, but you cannot drill or tap it: the same carbides that resist the abrasive destroy carbide drills and work-hardened taps within a few holes. The workable sequence is cast, soften, machine the fits and threads, then harden. It costs an extra heat cycle and it introduces distortion after machining, so the drawing has to carry enough stock on the machined faces to absorb it \u2014 the same logic we set out in the <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/ru\/%d0%b1%d0%bb%d0%be%d0%b3\/casting-machining-allowance\/\" target=\"_blank\" rel=\"noopener\">casting machining allowance<\/a> guide, applied to a material that moves more than most. Fits that have to hold a tolerance are normally finished after hardening in a <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/ru\/cnc-machining-services\/\" target=\"_blank\" rel=\"noopener\">CNC machining services<\/a> cell set up for hard turning and grinding.<\/p>\n<h2 style=\"font-family: 'Poppins',sans-serif; color: #273171; font-size: 25px; font-weight: 600; line-height: 1.3; margin: 34px 0 14px; padding: 4px 0 4px 30px; background: linear-gradient(to right, #ff512f 0px, #dd2476 5px, transparent 5px);\">Where White Iron Wear Parts Fail: Four Modes That Decide the Grade<\/h2>\n<p style=\"margin: 0 0 18px;\">Wear is not one phenomenon, and the grade that wins one test loses another. For high chrome white iron castings four modes decide the specification.<\/p>\n<ul style=\"margin: 0 0 18px; padding-left: 22px;\">\n<li style=\"margin: 0 0 8px;\"><strong style=\"color: #273171;\">Low-stress scratching.<\/strong> Fine particles sliding at speed: slurry lines, chute liners, fan blades, dredge pipe. The abrasive does not fracture the carbide, it scratches the matrix between carbides and eventually undermines them. 25\u201327% Cr at 600\u2013650 HB is the standard answer, and carbide volume fraction is what buys life.<\/li>\n<li style=\"margin: 0 0 8px;\"><strong style=\"color: #273171;\">High-stress grinding.<\/strong> The particle is crushed between two metal surfaces: roller press rolls, ball mill liners, jaw and cone wear plates. Now the carbide is loaded directly and can crack, so the matrix has to support it. 15\u201320% Cr with molybdenum, or 26% Cr at lower carbon, survives better than the hardest grade available.<\/li>\n<li style=\"margin: 0 0 8px;\"><strong style=\"color: #273171;\">Impact.<\/strong> Any blow that stores enough energy to propagate a crack through the carbide network. Above a certain energy level, no white iron is the right answer and the specification should move to Hadfield manganese steel or a martensitic steel.<\/li>\n<li style=\"margin: 0 0 8px;\"><strong style=\"color: #273171;\">Erosion-corrosion.<\/strong> Slurry that is also acidic or chloride-bearing, as in flue-gas desulfurisation and some phosphate duty. Chromium in solution protects the matrix, so the answer is 28\u201330% Cr even though abrasion resistance is slightly lower than at 26%.<\/li>\n<\/ul>\n<table style=\"width: 100%; border-collapse: collapse; margin: 18px 0 24px; font-size: 15px; color: #333333;\">\n<thead>\n<tr>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Wear mode<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Governing property<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Grade that usually wins<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Common wrong choice<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Low-stress scratching<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Carbide volume fraction<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">26% Cr, 2.8\u20133.2% C, hardened \u2265600 HB<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">12% Cr sold as equivalent<\/td>\n<\/tr>\n<tr style=\"background: #F5F5F5;\">\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">High-stress grinding<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Carbide support by matrix<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">20% Cr \u2013 1% Mo, or 26% Cr at 2.5% C<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Maximum-carbon hypereutectic<\/td>\n<\/tr>\n<tr>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Impact<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Fracture toughness<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Hadfield Mn steel, or quenched and tempered martensitic steel<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Any white iron<\/td>\n<\/tr>\n<tr style=\"background: #F5F5F5;\">\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Erosion-corrosion<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Cr in solid solution<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">28\u201330% Cr<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Ni-Hard, 12% Cr<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<h2 style=\"font-family: 'Poppins',sans-serif; color: #273171; font-size: 25px; font-weight: 600; line-height: 1.3; margin: 34px 0 14px; padding: 4px 0 4px 30px; background: linear-gradient(to right, #ff512f 0px, #dd2476 5px, transparent 5px);\">Design Rules for High Chrome White Iron Castings<\/h2>\n<p style=\"margin: 0 0 18px;\">High chrome white iron castings punish geometry that a ductile iron part would tolerate. Four rules cover most of the failures we see at the drawing review stage.<\/p>\n<h3 style=\"font-family: 'Poppins',sans-serif; color: #273171; font-size: 20px; font-weight: 600; line-height: 1.4; margin: 26px 0 8px; text-transform: capitalize;\">Minimum section and section uniformity<\/h3>\n<hr style=\"width: 100px; height: 4px; background: #EF890D; border: none; border-radius: 2px; margin: 0 0 14px; line-height: 0; opacity: 1;\" \/>\n<p style=\"margin: 0 0 18px;\">Below about 15\u201320 mm, a high chrome white iron casting chills against the mould, develops a continuous carbide skin and cracks either at shakeout or in the first thermal cycle of service. Junctions where a 60 mm boss meets a 15 mm wall are worse: the heavy section arrives late, the light section is already rigid, and the shrinkage stress has nowhere to go. Generous fillets \u2014 12 mm radius minimum, more at internal corners \u2014 and gradual transitions do more for service life than another two points of hardness.<\/p>\n<h3 style=\"font-family: 'Poppins',sans-serif; color: #273171; font-size: 20px; font-weight: 600; line-height: 1.4; margin: 26px 0 8px; text-transform: capitalize;\">Contraction allowance<\/h3>\n<hr style=\"width: 100px; height: 4px; background: #EF890D; border: none; border-radius: 2px; margin: 0 0 14px; line-height: 0; opacity: 1;\" \/>\n<p style=\"margin: 0 0 18px;\">White iron contracts about 2.0\u20132.4% linearly on solidification and cooling. Gray iron, because graphite precipitation offsets part of the contraction, needs only about 1.0%. Reuse a gray iron pattern for a high-chrome part and the arithmetic is unforgiving: a pattern cut for a 600 mm nominal dimension with a 1.0% allowance is 606.0 mm long, and a metal that actually contracts 2.2% produces a casting of 592.9 mm \u2014 7 mm undersize, which no as-cast tolerance grade for a 600 mm dimension can absorb. The pattern has to be cut, or re-cut, for the alloy, which is one of the reasons <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/ru\/casting-molds-making\/\" target=\"_blank\" rel=\"noopener\">mould and pattern making<\/a> for a new wear part is not a trivial line item.<\/p>\n<h3 style=\"font-family: 'Poppins',sans-serif; color: #273171; font-size: 20px; font-weight: 600; line-height: 1.4; margin: 26px 0 8px; text-transform: capitalize;\">Feeding and yield<\/h3>\n<hr style=\"width: 100px; height: 4px; background: #EF890D; border: none; border-radius: 2px; margin: 0 0 14px; line-height: 0; opacity: 1;\" \/>\n<p style=\"margin: 0 0 18px;\">High chrome white iron castings feed badly. The freezing range is narrow, the feeding distance is short, and the part cannot be patched afterwards. Take a 300 \u00d7 200 \u00d7 40 mm wear block: 2,400 cm\u00b3 of volume against 1,600 cm\u00b2 of cooling surface gives a modulus of 1.50 cm. A riser sized at 1.2 times that modulus needs M = 1.80 cm, which for a cylindrical riser with height equal to diameter means 108 mm diameter and about 989 cm\u00b3 of metal that ships as scrap. Yield lands near 71%, so every finished kilogram was poured as 1.41 kg. That single ratio explains most of the price gap against a steel plate, and it is worth understanding before arguing about the rate per kilogram.<\/p>\n<h3 style=\"font-family: 'Poppins',sans-serif; color: #273171; font-size: 20px; font-weight: 600; line-height: 1.4; margin: 26px 0 8px; text-transform: capitalize;\">No weld repair, so the process gate does the work<\/h3>\n<hr style=\"width: 100px; height: 4px; background: #EF890D; border: none; border-radius: 2px; margin: 0 0 14px; line-height: 0; opacity: 1;\" \/>\n<p style=\"margin: 0 0 18px;\">A532 high-chrome castings are not weld-repaired. Pump OEM purchase specifications state it explicitly \u2014 no weld repairs allowed \u2014 and the metallurgical reason is sound: welding a 600 HB carbide-bearing iron produces a brittle heat-affected zone that fails in service, and even a cosmetically acceptable repair leaves a stress raiser in a part whose whole job is to resist cracking. That is the opposite of the situation for <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/ru\/%d0%b1%d0%bb%d0%be%d0%b3\/casting-weld-repair\/\" target=\"_blank\" rel=\"noopener\">casting weld repair<\/a> in carbon and low-alloy steel, where a qualified procedure under ASTM A488 is normal practice. The consequence for a buyer is that the quality gate has to sit upstream: pattern, gating, pouring temperature, shakeout time, and a hardness map that shows the part was actually through-hardened.<\/p>\n<h2 style=\"font-family: 'Poppins',sans-serif; color: #273171; font-size: 25px; font-weight: 600; line-height: 1.3; margin: 34px 0 14px; padding: 4px 0 4px 30px; background: linear-gradient(to right, #ff512f 0px, #dd2476 5px, transparent 5px);\">Heat Treatment: Getting a White Iron Part to 600 HB<\/h2>\n<p style=\"margin: 0 0 18px;\">An as-cast 26% Cr high chrome white iron casting usually lands between 450 and 550 HB. That is enough for a chute liner and not enough for a slurry pump impeller. The step up comes from destabilisation: hold the casting at roughly 980\u20131,020 \u00b0C for a time scaled to section \u2014 commonly two hours plus one hour per 25 mm \u2014 then air cool. That cycle precipitates secondary carbide from the austenite and leaves a martensitic matrix on cooling. A temper at 200\u2013250 \u00b0C follows, mainly to relieve the stress the quench put in, not to soften.<\/p>\n<p style=\"margin: 0 0 18px;\">The failure mode to watch in high chrome white iron castings is retained austenite in heavy sections. Cool a 150 mm hub in still air and the core may not transform; the part then reads soft on the bench, hardens further under load in service, grows a few thousandths of a millimetre, and spalls. Molybdenum, copper and nickel additions in the A532 window exist partly to buy hardenability for that reason, which is why the same class can be specified with different alloy additions for a 25 mm liner and a 150 mm casing. The heat-treatment basics are shared with other alloys \u2014 our <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/ru\/%d0%b1%d0%bb%d0%be%d0%b3\/%d1%82%d0%b5%d1%80%d0%bc%d0%be%d0%be%d0%b1%d1%80%d0%b0%d0%b1%d0%be%d1%82%d0%ba%d0%b0-%d0%be%d1%82%d0%bb%d0%b8%d0%b2%d0%be%d0%ba\/\" target=\"_blank\" rel=\"noopener\">\u0442\u0435\u0440\u043c\u043e\u043e\u0431\u0440\u0430\u0431\u043e\u0442\u043a\u0430 \u043e\u0442\u043b\u0438\u0432\u043e\u043a<\/a> article covers the cycles \u2014 but the acceptance criterion here is a hardness figure in a specific place.<\/p>\n<p style=\"margin: 0 0 18px;\">Because hardness is a through-section property that changes with position, and because high chrome white iron castings have no repair route, the acceptance test should specify: the method (Brinell, typically 10 mm ball, 3,000 kgf), the location (on the casting surface or up to 3 mm below it, as the standard allows), the number of readings, and whether the reading is taken on the part or on a test block cast from the same ladle. A single reading on a polished pad in the thinnest section is not evidence of a through-hardened casting, and it is the most common way a cheap supplier passes a hardness clause that a good one would also pass honestly.<\/p>\n<figure style=\"margin: 24px 0;\"><img decoding=\"async\" style=\"width: 100%; display: block; border-radius: 4px;\" src=\"https:\/\/chinametalfoundry.com\/wp-content\/uploads\/2026\/11\/p252-hcwi-liners.webp\" alt=\"Worn and new high chrome white iron castings wear liner plates side by side\" \/><figcaption style=\"font-size: 13px; color: #7e7e7e; text-align: center; margin-top: 8px;\">Worn and replacement high chrome white iron castings: liner thickness is the measurement that sets the change-out interval, and it is what the cost-per-hour model uses.<\/figcaption><\/figure>\n<h2 style=\"font-family: 'Poppins',sans-serif; color: #273171; font-size: 25px; font-weight: 600; line-height: 1.3; margin: 34px 0 14px; padding: 4px 0 4px 30px; background: linear-gradient(to right, #ff512f 0px, #dd2476 5px, transparent 5px);\">Cost per Operating Hour, Not Cost per Kilogram<\/h2>\n<p style=\"margin: 0 0 18px;\">The quotation that matters compares two alloys on the same duty over the same period. Price per kilogram is the least useful number in the file, because it ignores how long the part lasts and what it costs to change it. For high chrome white iron castings the only comparable metric is cost per operating hour.<\/p>\n<h3 style=\"font-family: 'Poppins',sans-serif; color: #273171; font-size: 20px; font-weight: 600; line-height: 1.4; margin: 26px 0 8px; text-transform: capitalize;\">Case A: chute liner plate, 800 \u00d7 600 \u00d7 20 mm<\/h3>\n<hr style=\"width: 100px; height: 4px; background: #EF890D; border: none; border-radius: 2px; margin: 0 0 14px; line-height: 0; opacity: 1;\" \/>\n<p style=\"margin: 0 0 18px;\">Volume is 9,600 cm\u00b3, which at 7.6 g\/cm\u00b3 is 73.0 kg. At $4.35\/kg finished in the hardened condition, the high chrome white iron casting costs $317.38. A quenched and tempered 450 HB wear steel plate of the same size costs $141.09 \u2014 2.2 times less. On a straight price comparison the steel wins and the conversation ends there, which is the mistake.<\/p>\n<p style=\"margin: 0 0 18px;\">Assume the duty data from a typical aggregate chute: the high-chrome plate runs 5,600 hours, the 450 HB steel plate 950 hours. Changing a liner takes two fitters about five hours plus five hours of production stoppage, which we cost at $1,980 per change. Over 10,000 operating hours the high-chrome plate is changed 1.79 times and the steel plate 10.5 times.<\/p>\n<table style=\"width: 100%; border-collapse: collapse; margin: 18px 0 24px; font-size: 15px; color: #333333;\">\n<thead>\n<tr>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Per 10,000 operating hours<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">26% Cr white iron<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">450 HB wear steel<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Part price<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">$317.38<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">$141.09<\/td>\n<\/tr>\n<tr style=\"background: #F5F5F5;\">\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Wear life<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">5,600 h<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">950 h<\/td>\n<\/tr>\n<tr>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Changes required<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">1.79<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">10.5<\/td>\n<\/tr>\n<tr style=\"background: #F5F5F5;\">\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Parts spend<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">$566.74<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">$1,485.14<\/td>\n<\/tr>\n<tr>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Change-out labour and downtime<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">$3,535.72<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">$20,842.10<\/td>\n<\/tr>\n<tr style=\"background: #F5F5F5;\">\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">\u0418\u0442\u043e\u0433\u043e<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">$4,102.46<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">$22,327.24<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p style=\"margin: 0 0 18px;\">The high-chrome plate costs 2.2 times more to buy and 5.4 times less to run. Note where the money goes: even on parts alone the white iron is cheaper per hour, because the life ratio of 5.9 beats the price ratio of 2.2. The downtime line then widens the gap to the point where the alloy choice is no longer a procurement decision, it is an availability decision.<\/p>\n<h3 style=\"font-family: 'Poppins',sans-serif; color: #273171; font-size: 20px; font-weight: 600; line-height: 1.4; margin: 26px 0 8px; text-transform: capitalize;\">Case B: slurry pump impeller, 38 kg, 26% Cr against 12% Cr<\/h3>\n<hr style=\"width: 100px; height: 4px; background: #EF890D; border: none; border-radius: 2px; margin: 0 0 14px; line-height: 0; opacity: 1;\" \/>\n<p style=\"margin: 0 0 18px;\">Here both options are white iron, so the comparison is inside the family. At $4.90\/kg plus $118 of machining, the 26% Cr high chrome white iron casting comes to $304.20 and runs 4,200 hours. A 12% Cr impeller at $4.10\/kg comes to $273.80 and runs 2,600 hours. The premium is $30.40, or 11% on the part.<\/p>\n<p style=\"margin: 0 0 18px;\">Cost per 1,000 operating hours is $72.43 for the 26% Cr part against $105.31 for the 12% Cr part, a 31% reduction. The $30.40 premium is recovered after 925 operating hours \u2014 less than a quarter of the 26% Cr part\u2019s own life. Any pump that runs more than about five weeks a year should be on the higher-chrome grade, and the only situation where the cheaper impeller makes sense is a pump that is idle most of the year or is about to be replaced.<\/p>\n<p style=\"margin: 0 0 18px;\">This is the same structure as any other total-cost argument on the site: the <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/ru\/%d0%b1%d0%bb%d0%be%d0%b3\/casting-total-cost-of-ownership\/\" target=\"_blank\" rel=\"noopener\">casting total cost of ownership<\/a> logic applies directly, and the <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/ru\/%d0%b1%d0%bb%d0%be%d0%b3\/%d1%80%d0%b0%d0%b7%d0%b1%d0%b8%d0%b2%d0%ba%d0%b0-%d0%b7%d0%b0%d1%82%d1%80%d0%b0%d1%82-%d0%bd%d0%b0-%d0%bb%d0%b8%d1%82%d1%8c%d0%b5\/\" target=\"_blank\" rel=\"noopener\">\u0440\u0430\u0437\u0431\u0438\u0432\u043a\u0430 \u0437\u0430\u0442\u0440\u0430\u0442 \u043d\u0430 \u043b\u0438\u0442\u044c\u0435<\/a> article shows how the per-kilogram figure is actually built, riser yield included.<\/p>\n<figure style=\"margin: 24px 0;\"><img decoding=\"async\" style=\"width: 100%; display: block; border-radius: 4px;\" src=\"https:\/\/chinametalfoundry.com\/wp-content\/uploads\/2026\/11\/p252-hcwi-hardness.webp\" alt=\"Hardness testing of a high chrome white iron castings wear block on a Brinell tester\" \/><figcaption style=\"font-size: 13px; color: #7e7e7e; text-align: center; margin-top: 8px;\">Hardness acceptance on high chrome white iron castings: the reading, the location and the test block all belong in the specification.<\/figcaption><\/figure>\n<h2 style=\"font-family: 'Poppins',sans-serif; color: #273171; font-size: 25px; font-weight: 600; line-height: 1.3; margin: 34px 0 14px; padding: 4px 0 4px 30px; background: linear-gradient(to right, #ff512f 0px, #dd2476 5px, transparent 5px);\">When a White Iron Part Is the Wrong Choice<\/h2>\n<p style=\"margin: 0 0 18px;\">Roughly one enquiry in four that arrives asking for high chrome white iron castings should be something else. The disqualifiers are specific:<\/p>\n<ul style=\"margin: 0 0 18px; padding-left: 22px;\">\n<li style=\"margin: 0 0 8px;\"><strong style=\"color: #273171;\">The part takes a real impact.<\/strong> Crusher hammers, jaw plates, grizzly bars struck by oversize rock, and anything downstream of a tramp-metal risk. A 26% Cr part that chips in the first week is more expensive than a Hadfield manganese part that work-hardens from about 200 HB to 450\u2013500 HB under the same blows and tolerates large plastic deformation instead of cracking.<\/li>\n<li style=\"margin: 0 0 8px;\"><strong style=\"color: #273171;\">The section is thin.<\/strong> Below 15 mm, or a thin web between two heavy bosses, the part will crack in heat treatment as often as in service. Redesign the geometry before changing the alloy.<\/li>\n<li style=\"margin: 0 0 8px;\"><strong style=\"color: #273171;\">Someone will want to repair it in the field.<\/strong> No weld repair is the rule, and a maintenance team with a welding set will try anyway. If a site cannot accept a scrap-and-replace policy, a steel or ductile iron part is the honest specification.<\/li>\n<li style=\"margin: 0 0 8px;\"><strong style=\"color: #273171;\">It needs tapped holes or fine bores in the hardened condition.<\/strong> Threads have to be cast in as steel inserts or produced before hardening. If the design cannot accommodate that, the alloy is wrong for the drawing.<\/li>\n<li style=\"margin: 0 0 8px;\"><strong style=\"color: #273171;\">The duty is corrosion with little abrasion.<\/strong> A 30% Cr iron helps, but a stainless or a rubber-lined part is usually cheaper and better. White iron is a wear solution, not a corrosion solution.<\/li>\n<\/ul>\n<table style=\"width: 100%; border-collapse: collapse; margin: 18px 0 24px; font-size: 15px; color: #333333;\">\n<thead>\n<tr>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Symptom in service<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Likely cause<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Correct response<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Cracks radiating from a boss or fillet within days<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Section modulus mismatch, no fillet<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Redesign transition; do not raise hardness<\/td>\n<\/tr>\n<tr style=\"background: #F5F5F5;\">\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Corner spalling on a hammer or jaw<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Impact energy beyond the alloy<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Move to Hadfield Mn steel or martensitic steel<\/td>\n<\/tr>\n<tr>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Wear rate far above expectation on a certified part<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Hardness measured in the wrong place, or matrix under-hardened<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Require a hardness map and a test block, per the <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/ru\/%d0%b1%d0%bb%d0%be%d0%b3\/%d0%bc%d0%b5%d1%82%d0%be%d0%b4%d1%8b-%d0%ba%d0%be%d0%bd%d1%82%d1%80%d0%be%d0%bb%d1%8f-%d0%bb%d0%b8%d1%82%d1%8c%d1%8f\/\" target=\"_blank\" rel=\"noopener\">inspection methods guide<\/a><\/td>\n<\/tr>\n<tr style=\"background: #F5F5F5;\">\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Even wear but a short interval<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Carbide volume too low for the particle size<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Raise carbon within the A532 window, or move from 12% to 26% Cr<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<h2 style=\"font-family: 'Poppins',sans-serif; color: #273171; font-size: 25px; font-weight: 600; line-height: 1.3; margin: 34px 0 14px; padding: 4px 0 4px 30px; background: linear-gradient(to right, #ff512f 0px, #dd2476 5px, transparent 5px);\">Specifying High Chrome White Iron Castings on the Purchase Order<\/h2>\n<p style=\"margin: 0 0 18px;\">Because the standard leaves a wide chemistry window for high chrome white iron castings, and no weld repair is available as a fallback, the purchase order carries most of the quality risk. Nine lines close almost all of it:<\/p>\n<ul style=\"margin: 0 0 18px; padding-left: 22px;\">\n<li style=\"margin: 0 0 8px;\"><strong style=\"color: #273171;\">Class, type and condition.<\/strong> Not &#8220;high chrome&#8221; \u2014 write A532 Class III Type A, hardened and stress relieved, \u2265600 HB.<\/li>\n<li style=\"margin: 0 0 8px;\"><strong style=\"color: #273171;\">Chemistry with a certificate.<\/strong> EN 10204 3.1, with carbon and the Cr:C ratio called out, not just the chromium range.<\/li>\n<li style=\"margin: 0 0 8px;\"><strong style=\"color: #273171;\">Hardness: method, location, count.<\/strong> Brinell, on the casting surface or up to 3 mm below, minimum three readings per part or one per test block, recorded.<\/li>\n<li style=\"margin: 0 0 8px;\"><strong style=\"color: #273171;\">Test block.<\/strong> Cast from the same ladle, same section, and shipped with the parts or retained with the heat number.<\/li>\n<li style=\"margin: 0 0 8px;\"><strong style=\"color: #273171;\">Repair policy.<\/strong> No weld repair, no impregnation of through-wall defects, no cosmetic filling.<\/li>\n<li style=\"margin: 0 0 8px;\"><strong style=\"color: #273171;\">Machining allowance and datum.<\/strong> State which faces are machined, how much stock, and whether the part is supplied softened for machining or hardened.<\/li>\n<li style=\"margin: 0 0 8px;\"><strong style=\"color: #273171;\">Dimensional standard.<\/strong> ISO 8062 grade, plus explicit tolerances on the wear faces that matter.<\/li>\n<li style=\"margin: 0 0 8px;\"><strong style=\"color: #273171;\">NDT where justified.<\/strong> Visual and dimensional on all parts; RT or UT on pump casings and anything with a pressure boundary.<\/li>\n<li style=\"margin: 0 0 8px;\"><strong style=\"color: #273171;\">First-article requirement.<\/strong> A full dimensional and hardness report on the first piece of each pattern, with the sampling rule defined.<\/li>\n<\/ul>\n<p style=\"margin: 0 0 18px;\">The RFQ itself is the earlier lever. A drawing that shows the wear surface, the particle size, the slurry concentration and the expected hours between changes will get a grade recommendation instead of a price; a drawing that says &#8220;wear resistant iron&#8221; will get whatever is cheapest to pour. Our <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/ru\/%d0%b1%d0%bb%d0%be%d0%b3\/casting-rfq\/\" target=\"_blank\" rel=\"noopener\">casting RFQ checklist<\/a> article lists the data a foundry needs, and the <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/ru\/%d0%b1%d0%bb%d0%be%d0%b3\/%d1%81%d0%be%d0%b3%d0%bb%d0%b0%d1%88%d0%b5%d0%bd%d0%b8%d0%b5-%d0%be-%d0%ba%d0%b0%d1%87%d0%b5%d1%81%d1%82%d0%b2%d0%b5-%d0%bb%d0%b8%d1%82%d1%8c%d1%8f\/\" target=\"_blank\" rel=\"noopener\">\u0441\u043e\u0433\u043b\u0430\u0448\u0435\u043d\u0438\u0435 \u043e \u043a\u0430\u0447\u0435\u0441\u0442\u0432\u0435 \u043b\u0438\u0442\u044c\u044f<\/a> covers the acceptance clauses that turn those data into something enforceable at receiving inspection.<\/p>\n<p style=\"margin: 0 0 18px;\">One more point on sourcing. High-chrome white iron is produced in quantity in China, but the capability spread is wide: induction melting and sand or shell moulding are common, controlled destabilisation and air quenching to a verified 600 HB across a heavy section are not. Ask for the hardness map from a previous heavy-section job before placing the first order, and if the duty is new or the wear mode is unclear, order a <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/ru\/%d1%83%d1%81%d0%bb%d1%83%d0%b3%d0%b8-%d0%bf%d0%be-%d0%bb%d0%b8%d1%82%d1%8c%d1%8e-%d0%bc%d0%b5%d1%82%d0%b0%d0%bb%d0%bb%d0%b8%d1%87%d0%b5%d1%81%d0%ba%d0%b8%d1%85-%d0%bf%d1%80%d0%be%d1%82%d0%be%d1%82\/\" target=\"_blank\" rel=\"noopener\">prototype casting run<\/a> in the production alloy rather than guessing from a data sheet. If the part is a replica of a worn original, the measuring work described in our <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/ru\/%d0%b1%d0%bb%d0%be%d0%b3\/casting-reverse-engineering\/\" target=\"_blank\" rel=\"noopener\">casting reverse engineering<\/a> article is the right starting point rather than a drawing traced by hand. A foundry group that pours iron castings across several processes, such as our own <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/ru\/%d1%80%d0%b5%d1%88%d0%b5%d0%bd%d0%b8%d1%8f\/%d1%87%d1%83%d0%b3%d1%83%d0%bd%d0%bd%d0%be%d0%b5-%d0%bb%d0%b8%d1%82%d1%8c%d0%b5\/\" target=\"_blank\" rel=\"noopener\">iron casting solutions<\/a>, can normally propose the grade and the heat treatment in one review instead of two.<\/p>\n<h2 style=\"font-family: 'Poppins',sans-serif; color: #273171; font-size: 25px; font-weight: 600; line-height: 1.3; margin: 34px 0 14px; padding: 4px 0 4px 30px; background: linear-gradient(to right, #ff512f 0px, #dd2476 5px, transparent 5px);\">\u0427\u0430\u0441\u0442\u043e \u0437\u0430\u0434\u0430\u0432\u0430\u0435\u043c\u044b\u0435 \u0432\u043e\u043f\u0440\u043e\u0441\u044b<\/h2>\n<h3 style=\"font-family: 'Poppins',sans-serif; color: #273171; font-size: 20px; font-weight: 600; line-height: 1.4; margin: 22px 0 8px;\">Can high chrome white iron castings be welded?<\/h3>\n<p style=\"margin: 0 0 18px;\">No. Above roughly 500 HB the carbide network and the martensitic matrix produce a brittle heat-affected zone, and A532 practice and OEM purchase specifications prohibit weld repair. Defects are handled by re-pouring, not by repair, which is why pattern and gating quality matters more here than in steel casting.<\/p>\n<h3 style=\"font-family: 'Poppins',sans-serif; color: #273171; font-size: 20px; font-weight: 600; line-height: 1.4; margin: 22px 0 8px;\">What hardness should I specify?<\/h3>\n<p style=\"margin: 0 0 18px;\">For pump internals, mill liners and chute liners, specify hardened and stress relieved at 600 HB minimum, measured by Brinell on the casting surface or up to 3 mm below it, with the number and location of readings stated. As-cast 450 HB is acceptable only for low-impact wear plate where the part is cheap relative to the change-out cost.<\/p>\n<h3 style=\"font-family: 'Poppins',sans-serif; color: #273171; font-size: 20px; font-weight: 600; line-height: 1.4; margin: 22px 0 8px;\">Is 26% Cr always better than 12% Cr?<\/h3>\n<p style=\"margin: 0 0 18px;\">For low-stress sliding abrasion, yes \u2014 in high chrome white iron castings the carbide volume and the M<sub>7<\/sub>C<sub>3<\/sub> structure give roughly 1.6 times the life at an 11% price premium on a typical impeller. For high-stress grinding, and for any duty with impact, the harder grade can lose, because the carbide cracks rather than wears.<\/p>\n<h3 style=\"font-family: 'Poppins',sans-serif; color: #273171; font-size: 20px; font-weight: 600; line-height: 1.4; margin: 22px 0 8px;\">How thick a section can be through-hardened?<\/h3>\n<p style=\"margin: 0 0 18px;\">It depends on the alloy additions, not only on chromium. A 26% Cr iron with molybdenum, copper and nickel will harden through 100 mm and beyond; the same analysis without them may retain austenite in a 60 mm core and read soft. Ask for the hardness at the heaviest section, measured on a sectioned test block, not at the surface.<\/p>\n<h3 style=\"font-family: 'Poppins',sans-serif; color: #273171; font-size: 20px; font-weight: 600; line-height: 1.4; margin: 22px 0 8px;\">Can the part be machined after hardening?<\/h3>\n<p style=\"margin: 0 0 18px;\">High chrome white iron castings can be ground and faced, yes, with cubic boron nitride or ceramic tooling. Drilling, tapping and reaming, no. The practical route is to cast, soften to 400 HB or below, machine the fits and threads, then harden \u2014 with enough stock on the machined faces to absorb the distortion of the second heat cycle.<\/p>\n<h3 style=\"font-family: 'Poppins',sans-serif; color: #273171; font-size: 20px; font-weight: 600; line-height: 1.4; margin: 22px 0 8px;\">What is the difference between high chrome white iron and Ni-Hard?<\/h3>\n<p style=\"margin: 0 0 18px;\">Ni-Hard is ASTM A532 Class I: about 4% nickel and 2% chromium, hardness typically in the 500\u2013600 HB range after hardening, cheaper on alloy cost and more forgiving to cast. High-chrome Class III replaces most of the nickel with 23\u201330% chromium, which produces harder M<sub>7<\/sub>C<sub>3<\/sub> carbides and much better corrosion resistance in slurry. For cement raw mill duty Ni-Hard is often adequate; for fine silica slurry at speed, the high-chrome grade lasts substantially longer.<\/p>\n<p style=\"margin: 0 0 18px;\">The short version: high chrome white iron castings are a wear calculation, not a material preference. Fix the wear mode first, then the carbon and chromium that produce the carbide volume for it, then the section geometry and heat treatment that let the part survive its own hardness. Price per kilogram falls out of that sequence almost automatically \u2014 and if it does not, the grade is wrong.<\/p>\n\t\t<div data-elementor-type=\"section\" data-elementor-id=\"3550\" class=\"elementor elementor-3550\" data-elementor-post-type=\"elementor_library\">\n\t\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-19b1acf1 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"19b1acf1\" data-element_type=\"section\" data-e-type=\"section\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;,&quot;ekit_has_onepagescroll_dot&quot;:&quot;yes&quot;}\">\n\t\t\t\t\t\t\t<div class=\"elementor-background-overlay\"><\/div>\n\t\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-56e26ed6\" data-id=\"56e26ed6\" data-element_type=\"column\" data-e-type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-52c3d00c elementor-widget elementor-widget-elementskit-heading\" data-id=\"52c3d00c\" data-element_type=\"widget\" data-e-type=\"widget\" data-settings=\"{&quot;ekit_we_effect_on&quot;:&quot;none&quot;}\" data-widget_type=\"elementskit-heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<div class=\"ekit-wid-con\" ><div class=\"ekit-heading elementskit-section-title-wraper text_left   ekit_heading_tablet-   ekit_heading_mobile-\"><h3 class=\"ekit-heading--title elementskit-section-title\">\u0418\u0449\u0435\u0442\u0435 \u043d\u0430\u0434\u0435\u0436\u043d\u044b\u0439 \u043c\u0435\u0442\u0430\u043b\u043b\u0443\u0440\u0433\u0438\u0447\u0435\u0441\u043a\u0438\u0439 \u0437\u0430\u0432\u043e\u0434 \u0432 \u041a\u0438\u0442\u0430\u0435?<\/h3><\/div><\/div>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-24c75aa0 elementor-widget elementor-widget-text-editor\" data-id=\"24c75aa0\" data-element_type=\"widget\" data-e-type=\"widget\" data-settings=\"{&quot;ekit_we_effect_on&quot;:&quot;none&quot;}\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<ul><li>\u041c\u044b \u043f\u043e\u043c\u043e\u0436\u0435\u043c \u0432\u0430\u043c \u043e\u043f\u0442\u0438\u043c\u0438\u0437\u0438\u0440\u043e\u0432\u0430\u0442\u044c \u043a\u043e\u043d\u0441\u0442\u0440\u0443\u043a\u0446\u0438\u044e \u0438\u0437\u0434\u0435\u043b\u0438\u044f \u0438 \u0441\u043e\u043a\u0440\u0430\u0442\u0438\u0442\u044c \u0440\u0430\u0441\u0445\u043e\u0434\u044b.<\/li><li>\u041c\u044b \u043c\u043e\u0436\u0435\u043c \u043f\u043e\u043c\u043e\u0447\u044c \u0432\u0430\u043c \u0441 \u0438\u0437\u0433\u043e\u0442\u043e\u0432\u043b\u0435\u043d\u0438\u0435\u043c \u0432\u044b\u0441\u043e\u043a\u043e\u043a\u0430\u0447\u0435\u0441\u0442\u0432\u0435\u043d\u043d\u044b\u0445 \u043b\u0438\u0442\u044b\u0445 \u0434\u0435\u0442\u0430\u043b\u0435\u0439 \u0432 \u0431\u043e\u043b\u044c\u0448\u0438\u0445 \u043e\u0431\u044a\u0435\u043c\u0430\u0445.<\/li><li>\u041c\u044b \u043c\u043e\u0436\u0435\u043c \u043e\u0441\u0443\u0449\u0435\u0441\u0442\u0432\u0438\u0442\u044c \u043f\u043e\u0441\u0442\u0430\u0432\u043a\u0443 \u0432\u043e\u0432\u0440\u0435\u043c\u044f \u0438 \u043f\u043e\u043b\u0443\u0447\u0438\u0442\u044c \u0431\u043e\u043b\u044c\u0448\u0435 \u0432\u043e\u0437\u043c\u043e\u0436\u043d\u043e\u0441\u0442\u0435\u0439 \u043d\u0430 \u0440\u044b\u043d\u043a\u0435 \u0441\u0431\u044b\u0442\u0430.<\/li><li>\u0412\u044b \u0441\u043c\u043e\u0436\u0435\u0442\u0435 \u0432\u043e\u0441\u043f\u043e\u043b\u044c\u0437\u043e\u0432\u0430\u0442\u044c\u0441\u044f \u0443\u0441\u043b\u0443\u0433\u0430\u043c\u0438 \u043a\u043e\u043c\u043f\u0430\u043d\u0438\u0438 Supro MFG \u043f\u043e \u043b\u0438\u0442\u044c\u044e \u043c\u0435\u0442\u0430\u043b\u043b\u043e\u0432.<\/li><\/ul>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-51a20937 elementor-align-left elementor-widget elementor-widget-global elementor-global-1143 elementor-widget-button\" data-id=\"51a20937\" data-element_type=\"widget\" data-e-type=\"widget\" data-settings=\"{&quot;ekit_we_effect_on&quot;:&quot;none&quot;}\" data-widget_type=\"button.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<div class=\"elementor-button-wrapper\">\n\t\t\t\t\t<a class=\"elementor-button elementor-button-link elementor-size-sm elementor-animation-grow\" href=\"https:\/\/chinametalfoundry.com\/ru\/%d0%ba%d0%be%d0%bd%d1%82%d0%b0%d0%ba%d1%82\/\">\n\t\t\t\t\t\t<span class=\"elementor-button-content-wrapper\">\n\t\t\t\t\t\t\t\t\t<span class=\"elementor-button-text\">\u0417\u0430\u043f\u0440\u043e\u0441\u0438\u0442\u044c \u0446\u0435\u043d\u0443 \u043d\u0430\u043f\u0440\u044f\u043c\u0443\u044e \u0441 \u0437\u0430\u0432\u043e\u0434\u0430 <\/span>\n\t\t\t\t\t<\/span>\n\t\t\t\t\t<\/a>\n\t\t\t\t<\/div>\n\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<\/div>\n\t\t\n<p class=\"sc-note\" style=\"font-size: 13px; color: #9a9a9a; margin: 28px 0 0;\">*Chemistry, hardness conditions and supply conditions referenced from ASTM A532\/A532M and from published pump-OEM purchase specifications; casting practice and cost figures from Supro MFG shop-floor records.<\/p>\n<\/article>","protected":false},"excerpt":{"rendered":"<p>High chrome white iron castings are bought for one reason: the part has to survive abrasive wear that eats mild [&hellip;]<\/p>\n","protected":false},"author":5,"featured_media":8189,"comment_status":"closed","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"default","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"","ast-breadcrumbs-content":"","ast-featured-img":"","footer-sml-layout":"","ast-disable-related-posts":"","theme-transparent-header-meta":"default","adv-header-id-meta":"","stick-header-meta":"default","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"set","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"var(--ast-global-color-4)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":""},"categories":[52],"tags":[46,47,50,42],"class_list":["post-8188","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-materials-alloys","tag-casting-materials","tag-casting-process","tag-casting-selection","tag-metal-casting"],"_links":{"self":[{"href":"https:\/\/chinametalfoundry.com\/ru\/wp-json\/wp\/v2\/posts\/8188","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/chinametalfoundry.com\/ru\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/chinametalfoundry.com\/ru\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/chinametalfoundry.com\/ru\/wp-json\/wp\/v2\/users\/5"}],"replies":[{"embeddable":true,"href":"https:\/\/chinametalfoundry.com\/ru\/wp-json\/wp\/v2\/comments?post=8188"}],"version-history":[{"count":4,"href":"https:\/\/chinametalfoundry.com\/ru\/wp-json\/wp\/v2\/posts\/8188\/revisions"}],"predecessor-version":[{"id":8207,"href":"https:\/\/chinametalfoundry.com\/ru\/wp-json\/wp\/v2\/posts\/8188\/revisions\/8207"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/chinametalfoundry.com\/ru\/wp-json\/wp\/v2\/media\/8189"}],"wp:attachment":[{"href":"https:\/\/chinametalfoundry.com\/ru\/wp-json\/wp\/v2\/media?parent=8188"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/chinametalfoundry.com\/ru\/wp-json\/wp\/v2\/categories?post=8188"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/chinametalfoundry.com\/ru\/wp-json\/wp\/v2\/tags?post=8188"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}