{"id":8718,"date":"2026-11-19T01:52:27","date_gmt":"2026-11-19T01:52:27","guid":{"rendered":"https:\/\/chinametalfoundry.com\/?p=8718"},"modified":"2026-11-20T07:14:05","modified_gmt":"2026-11-20T07:14:05","slug":"cope-lift-casting","status":"publish","type":"post","link":"https:\/\/chinametalfoundry.com\/pt\/blog\/cope-lift-casting\/","title":{"rendered":"Cope Lift in Casting: Calculating Flask Hold-Down Force and Preventing Runout"},"content":{"rendered":"<article class=\"sc-article\" style=\"max-width: 820px; margin: 0 auto; font-family: 'Poppins',sans-serif; color: #7e7e7e; font-size: 16px; line-height: 1.7;\">\n<div class=\"sc-intro\" style=\"background: #F5F5F5; border-radius: 20px; padding: 22px 24px; font-style: italic; color: #3a3a3a; margin: 0 0 26px; line-height: 1.6;\">\n<p style=\"margin: 0 0 18px;\"><strong style=\"color: #273171;\">Cope lift<\/strong> is the failure that looks like a cleaning problem but is actually a hydrostatic calculation. When molten metal pushes the upper flask half off the parting plane, you get a fin, a runout, or a scrapped casting \u2014 and the force behind it was fixed weeks earlier by the height of the pouring basin and the projected area of the cavity. This article gives you the arithmetic, the safety factors, and the eight fields to put in an RFQ.<\/p>\n<\/div>\n<p style=\"margin: 0 0 18px;\">Everything below comes from measurements on green-sand and no-bake flasks, cross-checked against alloy density data from the <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/www.aluminum.org\/\" target=\"_blank\" rel=\"noopener\">Aluminum Association<\/a> and the ductile iron specification <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/store.astm.org\/standards\/a536\" target=\"_blank\" rel=\"noopener\">ASTM A536<\/a>. We deliberately separate cope lift from core float \u2014 a different calculation covered in our <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/blog\/casting-mold-design-patterns\/\" target=\"_blank\" rel=\"noopener\">mold and pattern design guide<\/a> \u2014 and from ordinary parting-line flash. If you need the wider process context first, start with the <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/blog\/guia-de-fundicao-de-metais\/\" target=\"_blank\" rel=\"noopener\">guia de fundi\u00e7\u00e3o de metais<\/a> or our <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/fundicao-em-areia\/\" target=\"_blank\" rel=\"noopener\">sand casting service page<\/a>.<\/p>\n<figure style=\"margin: 24px 0;\"><img decoding=\"async\" style=\"width: 100%; display: block; border-radius: 4px;\" src=\"https:\/\/chinametalfoundry.com\/wp-content\/uploads\/2026\/11\/p269-cope-lift-1.webp\" alt=\"Cope lift in sand casting: weighted flask resting on a parting line\" \/><figcaption style=\"font-size: 13px; color: #7e7e7e; text-align: center; margin-top: 8px;\">Figure 1. A weighted upper flask: the hold-down mass must exceed the hydrostatic uplift.<\/figcaption><\/figure>\n<h2 style=\"font-family: 'Poppins',sans-serif; color: #273171; font-size: 25px; font-weight: 600; line-height: 1.3; margin: 34px 0 14px; padding: 4px 0 4px 30px; background: linear-gradient(to right, #ff512f 0px, #dd2476 5px, transparent 5px);\">1. What Cope Lift Actually Is \u2014 and What It Is Not<\/h2>\n<p style=\"margin: 0 0 18px;\">Cope lift is the vertical separation of the cope (upper mold half) from the drag (lower half) under ferrostatic pressure. The moment metal fills the cavity, it presses on every surface, including the horizontal ceiling of the cavity in the cope. That upward pressure acts over the projected area of the cavity at the parting plane. If the sum of the cope self-weight, the flask weight, and the applied hold-down force is smaller than that uplift, the joint opens. Metal flows into the gap. At best you get a fin to grind off; at worst you get a runout that empties the mold onto the floor.<\/p>\n<p style=\"margin: 0 0 18px;\">Three confusions cost buyers real money. First, <strong style=\"color: #273171;\">cope lift is not core float<\/strong>. A core is a low-density body immersed in a high-density fluid, so its net uplift is (\u03c1<sub>metal<\/sub> \u2212 \u03c1<sub>core<\/sub>) \u00d7 V<sub>core<\/sub> \u00d7 g, resisted by core prints and chaplets. Cope lift is \u03c1<sub>metal<\/sub> \u00d7 g \u00d7 h \u00d7 A, resisted by weights and clamps. Different geometry, different hardware, different sign convention on the sand density. Our <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/blog\/casting-mold-design-patterns\/\" target=\"_blank\" rel=\"noopener\">pattern design guide<\/a> works the core version; this article works the flask version.<\/p>\n<p style=\"margin: 0 0 18px;\">Second, cope lift is not &#8220;flash&#8221;. A thin, uniform parting-line fin usually means worn flask pins, a dirty joint face, or a slightly oversized cope seating \u2014 see <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/blog\/perfecting-sand-casting-parting-lines\/\" target=\"_blank\" rel=\"noopener\">parting line selection<\/a>. A cope lift fin is thick, wide, and typically heavier on the side nearest the sprue, because that is where the head is highest. Third, cope lift is not mold wall movement. Wall movement is a slow, elastic bulging of the sand face under the same pressure; we quantify it in Section 6.<\/p>\n<p style=\"margin: 0 0 18px;\">The practical reason to keep the categories separate is that the remedies do not transfer. Adding chaplets does nothing for cope lift. Re-machining flask pins does nothing for cope lift. Raising mold hardness does very little for cope lift, though it helps wall movement. The only things that stop cope lift are <strong style=\"color: #273171;\">mass, preload, and lower head<\/strong> \u2014 and of those three, mass is the one most often specified by habit rather than calculated. For a description of the sand system that produces the mold in the first place, see <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/blog\/green-sand-casting\/\" target=\"_blank\" rel=\"noopener\">green sand casting<\/a>.<\/p>\n<ul style=\"margin: 0 0 18px; padding-left: 22px;\">\n<li style=\"margin: 0 0 8px;\"><strong style=\"color: #273171;\">Uplift direction.<\/strong> Always normal to the parting plane, upward on the cope.<\/li>\n<li style=\"margin: 0 0 8px;\"><strong style=\"color: #273171;\">Driving variable.<\/strong> Effective head h measured from the parting plane to the free metal surface in the pouring basin, not the casting height.<\/li>\n<li style=\"margin: 0 0 8px;\"><strong style=\"color: #273171;\">Area that matters.<\/strong> Horizontal projection of cavity + runners + risers at the joint \u2014 not the surface area of the casting.<\/li>\n<li style=\"margin: 0 0 8px;\"><strong style=\"color: #273171;\">Typical failure.<\/strong> A single pour, not a trend. Once the joint opens, that mold is lost.<\/li>\n<\/ul>\n<h2 style=\"font-family: 'Poppins',sans-serif; color: #273171; font-size: 25px; font-weight: 600; line-height: 1.3; margin: 34px 0 14px; padding: 4px 0 4px 30px; background: linear-gradient(to right, #ff512f 0px, #dd2476 5px, transparent 5px);\">2. The Cope Lift Force Equation: Head \u00d7 Projected Area<\/h2>\n<p style=\"margin: 0 0 18px;\">Two equations do all the work. Ferrostatic pressure at the parting plane is <strong style=\"color: #273171;\">P = \u03c1 \u00b7 g \u00b7 h<\/strong>, and the uplift is <strong style=\"color: #273171;\">F = P \u00b7 A<\/strong>. Here \u03c1 is the density of the liquid alloy in kg\/m\u00b3, g is 9.81 m\/s\u00b2, h is the effective head in metres, and A is the projected horizontal area in m\u00b2. Note what is absent: casting weight, wall thickness, and pouring temperature. None of them appear.<\/p>\n<table style=\"width: 100%; border-collapse: collapse; margin: 18px 0 24px; font-size: 15px; color: #333333;\">\n<thead>\n<tr>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Alloy (liquid)<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">\u03c1 kg\/m\u00b3<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">P at h = 0.35 m, kPa<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">F at A = 0.30 m\u00b2, kN<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Equivalent mass, kg<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Gray iron, ASTM A48 Class 30<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">7,100<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">24.38<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">7.31<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">745<\/td>\n<\/tr>\n<tr style=\"background: #F5F5F5;\">\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Ductile iron, ASTM A536<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">7,200<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">24.72<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">7.42<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">756<\/td>\n<\/tr>\n<tr>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Cast steel, plain carbon<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">7,850<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">26.95<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">8.09<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">824<\/td>\n<\/tr>\n<tr style=\"background: #F5F5F5;\">\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Aluminium A356 \/ A380<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">2,400<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">8.24<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">2.47<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">252<\/td>\n<\/tr>\n<tr>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Tin bronze C83600<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">8,800<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">30.21<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">9.06<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">924<\/td>\n<\/tr>\n<tr style=\"background: #F5F5F5;\">\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Magnesium AZ91<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">1,800<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">6.18<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">1.85<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">189<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p style=\"margin: 0 0 18px;\">Table 1 is the first place buyers get surprised. The same flask and the same head produce 8.09 kN with cast steel but only 2.47 kN with A356 aluminium \u2014 a factor of 3.28. Density, not part weight, sets the load. Alloy density figures should be confirmed against the applicable specification (<a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/store.astm.org\/standards\/a536\" target=\"_blank\" rel=\"noopener\">ASTM A536<\/a> for ductile iron, the <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/www.aluminum.org\/\" target=\"_blank\" rel=\"noopener\">Aluminum Association<\/a> registers for aluminium) and measurement practice against <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/www.nist.gov\/topics\/metrology\" target=\"_blank\" rel=\"noopener\">NIST metrology guidance<\/a>.<\/p>\n<h3 style=\"font-family: 'Poppins',sans-serif; color: #273171; font-size: 20px; font-weight: 600; line-height: 1.4; margin: 26px 0 8px; text-transform: capitalize;\">Worked example: 800 \u00d7 600 mm flask<\/h3>\n<hr style=\"width: 100px; height: 4px; background: #EF890D; border: none; border-radius: 2px; margin: 0 0 14px; line-height: 0; opacity: 1;\" \/>\n<p style=\"margin: 0 0 18px;\">Take an 800 \u00d7 600 mm flask with a cavity, runner and riser whose combined horizontal projection at the joint is A = 0.30 m\u00b2. The pouring basin sits h = 0.35 m above the parting plane. For liquid iron at \u03c1 = 7,000 kg\/m\u00b3:<\/p>\n<ul style=\"margin: 0 0 18px; padding-left: 22px;\">\n<li style=\"margin: 0 0 8px;\"><strong style=\"color: #273171;\">Pressure.<\/strong> P = 7,000 \u00d7 9.81 \u00d7 0.35 = 24,034 Pa = 24.03 kPa.<\/li>\n<li style=\"margin: 0 0 8px;\"><strong style=\"color: #273171;\">Uplift.<\/strong> F = 24.03 kPa \u00d7 0.30 m\u00b2 = 7,210 N = 7.21 kN, or 735 kgf.<\/li>\n<li style=\"margin: 0 0 8px;\"><strong style=\"color: #273171;\">Cope self-weight.<\/strong> Sand 0.8 \u00d7 0.6 \u00d7 0.25 m \u00d7 1,550 kg\/m\u00b3 = 186 kg, plus a 60 kg steel half = 246 kg = 2.41 kN.<\/li>\n<li style=\"margin: 0 0 8px;\"><strong style=\"color: #273171;\">Net hold-down needed.<\/strong> 7.21 \u2212 2.41 = 4.80 kN, i.e. 489 kg of external mass with no safety factor.<\/li>\n<li style=\"margin: 0 0 8px;\"><strong style=\"color: #273171;\">With SF = 1.5.<\/strong> Total required resistance 10.82 kN = 1,102 kgf, so the extra ballast is about 856 kg.<\/li>\n<\/ul>\n<p style=\"margin: 0 0 18px;\">That 856 kg is a real materials-handling number, not a rounding exercise. It is roughly eight 107 kg cast-iron blocks, and it has to be placed symmetrically. Off-centre ballast creates a moment that opens one corner of the joint while the opposite corner stays tight \u2014 the classic &#8220;one-sided fin&#8221; that gets misdiagnosed as a worn flask. <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/blog\/sand-casting-tools-and-gating-system\/\" target=\"_blank\" rel=\"noopener\">Gating system design<\/a> fixes h; <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/blog\/casting-riser-design\/\" target=\"_blank\" rel=\"noopener\">riser sizing<\/a> fixes the riser footprint that contributes to A. Those two documents and this calculation should be reviewed together before tooling is cut.<\/p>\n<h3 style=\"font-family: 'Poppins',sans-serif; color: #273171; font-size: 20px; font-weight: 600; line-height: 1.4; margin: 26px 0 8px; text-transform: capitalize;\">Why a 20 kg casting can need more ballast than a 105 kg one<\/h3>\n<hr style=\"width: 100px; height: 4px; background: #EF890D; border: none; border-radius: 2px; margin: 0 0 14px; line-height: 0; opacity: 1;\" \/>\n<p style=\"margin: 0 0 18px;\">Because the driving term is projected area, not mass. Consider two iron parts poured in the same flask at the same head:<\/p>\n<table style=\"width: 100%; border-collapse: collapse; margin: 18px 0 24px; font-size: 15px; color: #333333;\">\n<thead>\n<tr>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Case<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Geometry<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Metal mass, kg<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Projected A, m\u00b2<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Uplift, kN<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">A \u2014 thin cover plate<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">800 \u00d7 600 \u00d7 6 mm<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">20.2<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">0.300<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">7.21<\/td>\n<\/tr>\n<tr style=\"background: #F5F5F5;\">\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">B \u2014 compact boss<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">300 \u00d7 250 \u00d7 200 mm<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">105.0<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">0.075<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">1.80<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p style=\"margin: 0 0 18px;\">The 20.2 kg plate generates 4.0\u00d7 the uplift of the 105.0 kg boss. This inversion is why large, flat, thin-walled covers and panels are notorious for runout even though they look &#8220;light&#8221;. A buyer who approves hold-down by casting weight will systematically under-ballast exactly the parts most at risk. If your supplier quotes by kilogram, cross-check the geometry with the <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/blog\/discriminacao-dos-custos-de-fundicao\/\" target=\"_blank\" rel=\"noopener\">discrimina\u00e7\u00e3o dos custos de fundi\u00e7\u00e3o<\/a> e <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/blog\/casting-price-per-kg\/\" target=\"_blank\" rel=\"noopener\">price per kg<\/a> frameworks, which explain where the mass-based shortcut comes from and why it breaks here.<\/p>\n<figure style=\"margin: 24px 0;\"><img decoding=\"async\" style=\"width: 100%; display: block; border-radius: 4px;\" src=\"https:\/\/chinametalfoundry.com\/wp-content\/uploads\/2026\/11\/p269-cope-lift-2.webp\" alt=\"Cope lift force: ferrostatic head acting on the underside of an upper mold half\" \/><figcaption style=\"font-size: 13px; color: #7e7e7e; text-align: center; margin-top: 8px;\">Figure 2. Head is measured to the free surface in the basin, not to the top of the casting.<\/figcaption><\/figure>\n<h2 style=\"font-family: 'Poppins',sans-serif; color: #273171; font-size: 25px; font-weight: 600; line-height: 1.3; margin: 34px 0 14px; padding: 4px 0 4px 30px; background: linear-gradient(to right, #ff512f 0px, #dd2476 5px, transparent 5px);\">3. Where the Head Comes From \u2014 and Why Riser Height Changes Cope Lift<\/h2>\n<p style=\"margin: 0 0 18px;\">Effective head h is the vertical distance from the parting plane to the highest free surface of liquid metal during pouring. In practice that is the pouring basin level while the sprue is running, or the top of an open riser once the cavity fills. It is not the casting height. A 150 mm tall casting poured through a 350 mm sprue sees 350 mm of head at the joint.<\/p>\n<table style=\"width: 100%; border-collapse: collapse; margin: 18px 0 24px; font-size: 15px; color: #333333;\">\n<thead>\n<tr>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Head h, mm<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">P, kPa<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Uplift, kN<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Equivalent mass, kg<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Ballast vs. 856 kg baseline<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">200<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">13.73<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">4.12<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">420<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">49%<\/td>\n<\/tr>\n<tr style=\"background: #F5F5F5;\">\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">250<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">17.17<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">5.15<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">525<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">61%<\/td>\n<\/tr>\n<tr>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">300<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">20.60<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">6.18<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">630<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">74%<\/td>\n<\/tr>\n<tr style=\"background: #F5F5F5;\">\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">350<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">24.03<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">7.21<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">735<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">86%<\/td>\n<\/tr>\n<tr>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">400<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">27.47<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">8.24<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">840<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">98%<\/td>\n<\/tr>\n<tr style=\"background: #F5F5F5;\">\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">450<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">30.90<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">9.27<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">945<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">110%<\/td>\n<\/tr>\n<tr>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">500<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">34.34<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">10.30<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">1,050<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">123%<\/td>\n<\/tr>\n<tr style=\"background: #F5F5F5;\">\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">550<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">37.77<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">11.33<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">1,155<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">135%<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p style=\"margin: 0 0 18px;\">Every additional 50 mm of head adds 1.03 kN, about 105 kgf, at A = 0.30 m\u00b2. That is a 14.3% jump in uplift for a change that a pourer can make by simply setting a taller pouring cup on the same flask. This is the second counter-intuitive result: <strong style=\"color: #273171;\">a feeding improvement can cause a structural failure<\/strong>. Raising an open riser to improve feeding increases h; adding a taller sprue to improve fill increases h; both add cope lift linearly, and neither normally triggers a review of the ballast chart.<\/p>\n<p style=\"margin: 0 0 18px;\">Coordinate the two decisions. <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/blog\/casting-riser-design\/\" target=\"_blank\" rel=\"noopener\">Riser design<\/a> determines the feeding modulus and riser height; <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/blog\/casting-pouring-temperature\/\" target=\"_blank\" rel=\"noopener\">pouring temperature windows<\/a> determines how much superheat you need; <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/blog\/casting-simulation\/\" target=\"_blank\" rel=\"noopener\">solidification simulation<\/a> flags the fill sequence. Any change to sprue or riser height should reopen the cope lift calculation. The same applies to <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/blog\/foundry-core-making\/\" target=\"_blank\" rel=\"noopener\">core making<\/a> changes that alter the cavity projection, and to tooling rework handled by <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/casting-molds-making\/\" target=\"_blank\" rel=\"noopener\">fabrico de moldes e modelos<\/a>. A useful discipline is to record h on the process sheet as a controlled variable, with the same status as pouring temperature.<\/p>\n<p style=\"margin: 0 0 18px;\">Lowering the basin is not a free fix. Reduce h too far and you lose the pressure needed to feed thin sections, inviting misruns and cold shuts; the <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/blog\/controlo-da-turbulencia-do-fluxo-na-fundicao-em-areia\/\" target=\"_blank\" rel=\"noopener\">flow turbulence control<\/a> e <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/blog\/sand-casting-tools-and-gating-system\/\" target=\"_blank\" rel=\"noopener\">sistema de controlo de acesso<\/a> guides explain the trade. The safe order is: calculate the required head for filling and feeding, then size the hold-down for that head \u2014 never the reverse.<\/p>\n<h2 style=\"font-family: 'Poppins',sans-serif; color: #273171; font-size: 25px; font-weight: 600; line-height: 1.3; margin: 34px 0 14px; padding: 4px 0 4px 30px; background: linear-gradient(to right, #ff512f 0px, #dd2476 5px, transparent 5px);\">4. Three Ways to Resist Cope Lift: Weights, Clamps and Flask Pins<\/h2>\n<p style=\"margin: 0 0 18px;\">Once F is known, resistance comes from four mechanisms. They are not interchangeable, and their failure modes differ enough that a supplier should be able to name which one is in use on a given job.<\/p>\n<table style=\"width: 100%; border-collapse: collapse; margin: 18px 0 24px; font-size: 15px; color: #333333;\">\n<thead>\n<tr>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Method<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Typical resistance<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">O mais adequado<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Dominant failure mode<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Added cost per mold<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Cast-iron ballast weights<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Any mass, 0.5\u20133 t typical<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Jobbing, large flasks, low volume<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Forgotten, off-centre, or shifted by vibration<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">0.8\u20131.5 min handling labour<\/td>\n<\/tr>\n<tr style=\"background: #F5F5F5;\">\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Flask clamps \/ bolted wedges<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">20\u201360 kN preload per M16\u2013M20 bolt<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Repeat production, high-pressure lines<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Preload relaxation, thread wear, flange bending<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">0.10\u20130.30 USD amortised fixture<\/td>\n<\/tr>\n<tr>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Pins + tapered wedges<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">5\u201315 kN per pair<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Small-to-medium flasks, fast changeover<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Pin wear, wedge loosening<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">0.05\u20130.12 USD consumables<\/td>\n<\/tr>\n<tr style=\"background: #F5F5F5;\">\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Hydraulic \/ pneumatic hold-down<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">30\u2013100 kN<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Automated molding lines<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Pressure loss, seal leakage, interlock bypass<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Capex, not per-mold<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p style=\"margin: 0 0 18px;\">For short runs, ballast wins on simplicity: gravity does not leak, needs no maintenance, and is visible at a glance. For repeat work, clamps win on consistency \u2014 but only if preload is actually measured. <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/blog\/automatizacao-de-fundicoes\/\" target=\"_blank\" rel=\"noopener\">Automa\u00e7\u00e3o de fundi\u00e7\u00f5es<\/a> e <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/blog\/casting-capacity-reservation\/\" target=\"_blank\" rel=\"noopener\">capacity reservation<\/a> decisions usually determine which regime a job falls into; a part booked on a high-pressure line will inherit that line&#8217;s clamping hardware whether or not anyone recomputed the force.<\/p>\n<h3 style=\"font-family: 'Poppins',sans-serif; color: #273171; font-size: 20px; font-weight: 600; line-height: 1.4; margin: 26px 0 8px; text-transform: capitalize;\">Bolt preload is rarely the weak link \u2014 span is<\/h3>\n<hr style=\"width: 100px; height: 4px; background: #EF890D; border: none; border-radius: 2px; margin: 0 0 14px; line-height: 0; opacity: 1;\" \/>\n<p style=\"margin: 0 0 18px;\">At SF = 1.5, the example flask needs 10.82 kN of total resistance. The cope contributes 2.41 kN by itself, leaving 8.40 kN for the hardware: 2.10 kN per bolt with four clamps, 1.68 kN with five. A single M16 property-class 8.8 bolt is typically preloaded to 40\u201350 kN, so the bolts are over-specified by more than an order of magnitude. Yet flasks clamped with four bolts still show parting-line fins at mid-span. The reason is the distance between bolts: on an 800 mm edge, four evenly spaced bolts leave 267 mm of unsupported span; five leave 200 mm. Bending deflection scales with the fourth power of span, so moving from four to five clamps cuts mid-span opening by roughly (200\/267)\u2074 \u2248 0.31 \u2014 about a 69% reduction \u2014 for a 25% increase in hardware.<\/p>\n<p style=\"margin: 0 0 18px;\">This is why the useful specification is <strong style=\"color: #273171;\">maximum clamp pitch in mm<\/strong>, not bolt grade. Shops that hold pitch at 200\u2013250 mm report parting-line opening below 0.1 mm; at 267 mm and above, 0.2\u20130.6 mm is common. Put the pitch, the torque value, and the re-torque interval into the <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/blog\/casting-first-article-inspection\/\" target=\"_blank\" rel=\"noopener\">inspe\u00e7\u00e3o do primeiro artigo<\/a> record and the <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/blog\/foundry-audit-checklist\/\" target=\"_blank\" rel=\"noopener\">foundry audit checklist<\/a>. If the joint still opens, check flask flatness with a straightedge before blaming the clamps \u2014 a warped flask cannot be preloaded into flatness. Machining the joint face is a job for <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/cnc-machining-services\/\" target=\"_blank\" rel=\"noopener\">CNC machining services<\/a>, not for more torque.<\/p>\n<h2 style=\"font-family: 'Poppins',sans-serif; color: #273171; font-size: 25px; font-weight: 600; line-height: 1.3; margin: 34px 0 14px; padding: 4px 0 4px 30px; background: linear-gradient(to right, #ff512f 0px, #dd2476 5px, transparent 5px);\">5. Safety Factors for Cope Lift: Static, Dynamic and Impact Allowances<\/h2>\n<p style=\"margin: 0 0 18px;\">The static equation is a lower bound. Real pours add three things the equation omits: the transient surge when the sprue first fills, the reaction of escaping gas in poorly vented molds, and the vibration of a molding line or a crane-set flask. A safety factor is how those get priced into the ballast chart.<\/p>\n<table style=\"width: 100%; border-collapse: collapse; margin: 18px 0 24px; font-size: 15px; color: #333333;\">\n<thead>\n<tr>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Condition<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Recommended SF<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Why<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Typical verification<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Hand-poured, well-vented, small flask<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">1.3<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Low surge, low vibration<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Static calculation + visual ballast check<\/td>\n<\/tr>\n<tr style=\"background: #F5F5F5;\">\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Hand-poured, large or thin flat casting<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">1.5<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Larger A, longer pour, more surge<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Calculation + first-pour witness<\/td>\n<\/tr>\n<tr>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Crane-set flask, bottom-pour ladle<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">1.5\u20131.8<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Settling and impact on seating<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Torque \/ mass log per mold<\/td>\n<\/tr>\n<tr style=\"background: #F5F5F5;\">\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Automated high-pressure molding line<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">1.8\u20132.0<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Line vibration, cycle-to-cycle variation<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">SPC on flash thickness + clamp pressure<\/td>\n<\/tr>\n<tr>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Any mold with restricted venting<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">+0.2 on the above<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Gas back-pressure adds to the joint load<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Vent check + permeability record<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p style=\"margin: 0 0 18px;\">Two cautions. First, a safety factor applied to force is not the same as a safety factor applied to mass: the cope self-weight already contributes, so multiplying total ballast by 1.5 overstates what is needed, while multiplying only the net uplift by 1.5 understates it. Use F \u00d7 SF as the total resistance target, then subtract cope self-weight \u2014 exactly the sequence in Section 2. Second, gas back-pressure is the most commonly ignored term. A mold with blocked vents can see a transient joint load well above \u03c1ghA even at modest head; <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/blog\/green-sand-casting\/\" target=\"_blank\" rel=\"noopener\">green sand permeability<\/a> e <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/blog\/casting-mold-coating\/\" target=\"_blank\" rel=\"noopener\">refractory mold coating<\/a> both affect it.<\/p>\n<p style=\"margin: 0 0 18px;\">For control-plan purposes, treat the hold-down setting as a controlled process parameter under the same discipline as <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/www.aiag.org\/\" target=\"_blank\" rel=\"noopener\">AIAG-style process control<\/a> and log it per mold. Molten-metal safety is a separate obligation: a runout is a burn and fire hazard, and <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/www.nfpa.org\/\" target=\"_blank\" rel=\"noopener\">NFPA guidance<\/a> should drive the spill containment and PPE requirements around the pouring station. Supplier <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/blog\/auditoria-a-fornecedores-de-pecas-fundidas\/\" target=\"_blank\" rel=\"noopener\">audit<\/a> visits should ask to see the ballast chart, not just the finished casting.<\/p>\n<h2 style=\"font-family: 'Poppins',sans-serif; color: #273171; font-size: 25px; font-weight: 600; line-height: 1.3; margin: 34px 0 14px; padding: 4px 0 4px 30px; background: linear-gradient(to right, #ff512f 0px, #dd2476 5px, transparent 5px);\">6. Mold Wall Movement: The Slower Cousin of Cope Lift<\/h2>\n<p style=\"margin: 0 0 18px;\">Cope lift opens the joint suddenly. The same ferrostatic pressure also pushes the sand face outward gradually, a phenomenon called mold wall movement or mold swell. It does not scrap the casting in one pour; it shifts dimensions, adds metal, and quietly eats machining allowance across a whole production run. Buyers often discover it as a machining-cost drift rather than a foundry defect.<\/p>\n<table style=\"width: 100%; border-collapse: collapse; margin: 18px 0 24px; font-size: 15px; color: #333333;\">\n<thead>\n<tr>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Mold face condition<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Equivalent stiffness, kPa\/mm<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Wall movement at 24.03 kPa, mm<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Two-sided size gain, mm<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Extra metal, kg\/part<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Well-compacted, B-scale ~90<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">240<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">0.100<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">\u2014<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">baseline<\/td>\n<\/tr>\n<tr style=\"background: #F5F5F5;\">\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Soft spots, B-scale ~75<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">130<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">0.185<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">0.169<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">0.57<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p style=\"margin: 0 0 18px;\">At 12,000 molds a year, a 0.169 mm two-sided gain over 0.48 m\u00b2 of cavity surface adds about 0.57 kg of iron per casting. At 1.10 USD\/kg that is 7,517 USD\/year of metal alone; add 2,160 USD\/year of extra tooling and cycle time from the larger machining allowance, and the soft-mold penalty is roughly 9,677 USD\/year. This is a different loss mechanism from cope lift and it needs a different control: mold hardness and compaction uniformity, not more ballast.<\/p>\n<p style=\"margin: 0 0 18px;\">The controls live in the sand system. <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/blog\/foundry-sand-reclamation\/\" target=\"_blank\" rel=\"noopener\">Sand reclamation quality<\/a> sets the grain distribution and LOI that drive compactability; <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/blog\/green-sand-casting\/\" target=\"_blank\" rel=\"noopener\">green sand compactability and moisture bands<\/a> set the achievable hardness; <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/blog\/casting-mold-coating\/\" target=\"_blank\" rel=\"noopener\">mold coating<\/a> seals surface pores against penetration. Dimensionally, the resulting drift shows up against <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/blog\/guia-de-tolerancias-de-fundicao\/\" target=\"_blank\" rel=\"noopener\">ISO 8062 casting tolerances<\/a>, and downstream <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/blog\/tratamento-termico-de-pecas-fundidas\/\" target=\"_blank\" rel=\"noopener\">tratamento t\u00e9rmico<\/a> can amplify distortion if the as-cast wall is already heavy. When a dimensional complaint arrives, check hardness records before reaching for the clamp chart.<\/p>\n<h2 style=\"font-family: 'Poppins',sans-serif; color: #273171; font-size: 25px; font-weight: 600; line-height: 1.3; margin: 34px 0 14px; padding: 4px 0 4px 30px; background: linear-gradient(to right, #ff512f 0px, #dd2476 5px, transparent 5px);\">7. Defect Map: Separating Cope Lift from Flash, Swell and Mismatch<\/h2>\n<p style=\"margin: 0 0 18px;\">A fin at the parting line has at least four possible causes, and the corrective action for each is different. Misclassification is expensive because the wrong fix adds cost without removing the failure.<\/p>\n<table style=\"width: 100%; border-collapse: collapse; margin: 18px 0 24px; font-size: 15px; color: #333333;\">\n<thead>\n<tr>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Observed feature<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Most likely cause<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Discriminating check<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Corrective action<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Thick, tapering fin; heavier near sprue; metal on the floor<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Cope lift<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Compare ballast log with calculated F; check basin height<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Recalculate hold-down; lower h or add symmetric mass<\/td>\n<\/tr>\n<tr style=\"background: #F5F5F5;\">\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Thin uniform fin all around the joint<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Worn pins \/ dirty joint \/ poor seating<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Straightedge on flask faces; pin gauge<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Re-machine pins and joint faces; clean seating<\/td>\n<\/tr>\n<tr>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Local bulge, oversize walls, no fin<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Mold wall movement<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">B-scale hardness map of the mold face<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Restore compaction uniformity and moisture control<\/td>\n<\/tr>\n<tr style=\"background: #F5F5F5;\">\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Offset of features across the parting plane<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Mold shift \/ mismatch<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Measure datum offset on both halves<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Replace dowels; verify closing fixtures<\/td>\n<\/tr>\n<tr>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Fin plus surface roughness and burned-on sand<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Metal penetration, often with low hardness<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Permeability and coating thickness records<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\"><a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/blog\/casting-mold-coating\/\" target=\"_blank\" rel=\"noopener\">Refractory wash<\/a> and finer sand<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p style=\"margin: 0 0 18px;\">Radiographic and visual acceptance criteria should be agreed before the first article, using <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/store.astm.org\/standards\/e446\" target=\"_blank\" rel=\"noopener\">ASTM E446 reference radiographs<\/a> where applicable and the method mix in <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/blog\/metodos-de-inspecao-de-pecas-fundidas\/\" target=\"_blank\" rel=\"noopener\">m\u00e9todos de inspe\u00e7\u00e3o de pe\u00e7as fundidas<\/a>. Cope lift fins are usually removable by grinding, but the decision to salvage belongs in a written <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/blog\/casting-nonconformance\/\" target=\"_blank\" rel=\"noopener\">nonconformance<\/a> record, not on the shop floor. <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/blog\/casting-weld-repair\/\" target=\"_blank\" rel=\"noopener\">Weld repair<\/a> is sometimes proposed for runout-damaged castings; it does not address the hydrostatic cause and should never be treated as a corrective action. The <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/blog\/defeitos-comuns-na-fundicao-e-como-evita-los\/\" target=\"_blank\" rel=\"noopener\">defeitos comuns de fundi\u00e7\u00e3o<\/a> overview places all four mechanisms in one diagnostic tree.<\/p>\n<figure style=\"margin: 24px 0;\"><img decoding=\"async\" style=\"width: 100%; display: block; border-radius: 4px;\" src=\"https:\/\/chinametalfoundry.com\/wp-content\/uploads\/2026\/11\/p269-cope-lift-3.webp\" alt=\"Cope lift hold-down hardware: steel guide pins, a tapered wedge and clamp bolts\" \/><figcaption style=\"font-size: 13px; color: #7e7e7e; text-align: center; margin-top: 8px;\">Figure 3. Clamp pitch and joint flatness matter more than bolt grade.<\/figcaption><\/figure>\n<h2 style=\"font-family: 'Poppins',sans-serif; color: #273171; font-size: 25px; font-weight: 600; line-height: 1.3; margin: 34px 0 14px; padding: 4px 0 4px 30px; background: linear-gradient(to right, #ff512f 0px, #dd2476 5px, transparent 5px);\">8. The Cost of Cope Lift: Ballast, Handling and Scrap<\/h2>\n<p style=\"margin: 0 0 18px;\">Here is the arithmetic that usually changes a supplier&#8217;s mind. Take 12,000 molds a year with a 1.8% runout and parting-line-fin scrap rate, at 42 USD of lost value per scrapped casting (metal, melting, cleaning, and the re-make). That is 216 castings and 9,072 USD\/year.<\/p>\n<table style=\"width: 100%; border-collapse: collapse; margin: 18px 0 24px; font-size: 15px; color: #333333;\">\n<thead>\n<tr>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Item<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Before<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">After<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Delta<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Ballast per mold, kg<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">856<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">1,056<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">+200<\/td>\n<\/tr>\n<tr style=\"background: #F5F5F5;\">\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Handling time per mold, min<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">baseline<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">+0.4<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">+80 h\/year<\/td>\n<\/tr>\n<tr>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Handling cost, USD\/year<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">\u2014<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">2,240<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">+2,240<\/td>\n<\/tr>\n<tr style=\"background: #F5F5F5;\">\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Runout \/ fin scrap rate<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">1.8%<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">0.4%<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">\u22121.4 pts<\/td>\n<\/tr>\n<tr>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Scrap loss, USD\/year<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">9,072<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">2,016<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">\u22127,056<\/td>\n<\/tr>\n<tr style=\"background: #F5F5F5;\">\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Net annual result, USD<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">\u2014<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">\u2014<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">+4,816<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p style=\"margin: 0 0 18px;\">Adding 200 kg of ballast costs 2,240 USD\/year in handling and saves 7,056 USD\/year in scrap: a net 4,816 USD\/year with essentially zero capital expenditure. The counter-intuitive part is not that ballast is cheap \u2014 it is that <strong style=\"color: #273171;\">the expensive failure was procedural, not mechanical<\/strong>. In most runout investigations the flask had enough total mass on the chart; it was placed off-centre, omitted on a night shift, or never re-checked after a riser was made taller. Writing the exact block count, positions, and a first-pour sign-off into the work instruction costs less than any hardware upgrade.<\/p>\n<p style=\"margin: 0 0 18px;\">By contrast, converting the job to bolted clamps might cost 18,000 USD in fixtures and save the 2,240 USD\/year of ballast handling \u2014 a 8.0-month payback on labour alone. But if the underlying failure was a missing block rather than insufficient force, the clamp conversion buys speed, not quality. Sequence matters: stabilise the procedure first, then automate it. The <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/blog\/casting-scrap-rate\/\" target=\"_blank\" rel=\"noopener\">scrap rate<\/a>, <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/blog\/casting-price-per-kg\/\" target=\"_blank\" rel=\"noopener\">price per kg<\/a> e <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/blog\/discriminacao-dos-custos-de-fundicao\/\" target=\"_blank\" rel=\"noopener\">cost breakdown<\/a> analyses show the same pattern in other cost centres, and <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/blog\/casting-defect-claim\/\" target=\"_blank\" rel=\"noopener\">defect claims<\/a> should record which mechanism was actually at fault. Prototype runs through <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/servicos-de-fundicao-de-prototipos-metalicos\/\" target=\"_blank\" rel=\"noopener\">prototipagem r\u00e1pida<\/a> are the cheapest place to validate a new hold-down arrangement before committing production tooling.<\/p>\n<h2 style=\"font-family: 'Poppins',sans-serif; color: #273171; font-size: 25px; font-weight: 600; line-height: 1.3; margin: 34px 0 14px; padding: 4px 0 4px 30px; background: linear-gradient(to right, #ff512f 0px, #dd2476 5px, transparent 5px);\">9. What to Ask a Foundry About Cope Lift: An Eight-Field RFQ Checklist<\/h2>\n<p style=\"margin: 0 0 18px;\">Most RFQs specify alloy, grade, tolerance and quantity, then leave the mold entirely unspecified. That is why two suppliers can quote the same drawing with very different runout risk. Eight fields close the gap.<\/p>\n<table style=\"width: 100%; border-collapse: collapse; margin: 18px 0 24px; font-size: 15px; color: #333333;\">\n<thead>\n<tr>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">#<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Field to require<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Why it matters<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Acceptable answer<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">1<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Projected area at parting plane, mm\u00b2<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Sets A in F = \u03c1ghA<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">A stated number, including runners and risers<\/td>\n<\/tr>\n<tr style=\"background: #F5F5F5;\">\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">2<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Effective ferrostatic head, mm<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Sets h; the most-often-changed variable<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Basin and open-riser levels on the process sheet<\/td>\n<\/tr>\n<tr>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">3<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Liquid alloy density, kg\/m\u00b3<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Changes load by up to 3.7\u00d7 across alloys<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Grade-specific value with the standard it came from<\/td>\n<\/tr>\n<tr style=\"background: #F5F5F5;\">\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">4<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Calculated uplift, kN<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Shows the arithmetic was actually done<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">F with A and h shown, not just &#8220;we use weights&#8221;<\/td>\n<\/tr>\n<tr>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">5<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Hold-down method and total resistance, kN<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Distinguishes mass, preload and pins<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Method + measured or rated resistance<\/td>\n<\/tr>\n<tr style=\"background: #F5F5F5;\">\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">6<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Safety factor and clamp pitch, mm<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Catches the mid-span failure mode<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">SF \u2265 1.5 and pitch \u2264 250 mm for repeat work<\/td>\n<\/tr>\n<tr>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">7<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Parting-line fin limit and measurement method<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Makes acceptance objective<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">A mm limit, gauge or caliper, at defined locations<\/td>\n<\/tr>\n<tr style=\"background: #F5F5F5;\">\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">8<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Runout scrap rate, last 12 months, and corrective actions<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Reveals whether the loop is closed<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">A rate plus dated actions tied to root cause<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p style=\"margin: 0 0 18px;\">Put these in the <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/blog\/casting-rfq\/\" target=\"_blank\" rel=\"noopener\">RFQ<\/a> template alongside the commercial terms in <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/blog\/acordo-de-qualidade-de-fundicao\/\" target=\"_blank\" rel=\"noopener\">the quality agreement<\/a> and verify them during a <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/blog\/auditoria-a-fornecedores-de-pecas-fundidas\/\" target=\"_blank\" rel=\"noopener\">supplier audit<\/a> or <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/blog\/casting-incoming-inspection-plan\/\" target=\"_blank\" rel=\"noopener\">incoming inspection<\/a> review. Keep the density assumption alloy-specific: our <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/solucoes\/fundicao-de-aluminio\/\" target=\"_blank\" rel=\"noopener\">aluminium casting solutions<\/a> e <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/solucoes\/steel-casting\/\" target=\"_blank\" rel=\"noopener\">steel casting solutions<\/a> pages cover the density and feeding differences, and the <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/www.aluminum.org\/\" target=\"_blank\" rel=\"noopener\">Aluminum Association<\/a> publications are the reference for aluminium grades. A supplier who can answer fields 1\u20134 in writing is usually the one who has instrumented the process rather than inherited a ballast habit.<\/p>\n<h2 style=\"font-family: 'Poppins',sans-serif; color: #273171; font-size: 25px; font-weight: 600; line-height: 1.3; margin: 34px 0 14px; padding: 4px 0 4px 30px; background: linear-gradient(to right, #ff512f 0px, #dd2476 5px, transparent 5px);\">10. A 30-Day Plan to Close the Cope Lift Loop<\/h2>\n<p style=\"margin: 0 0 18px;\">For a part already in production, the fix does not require new tooling. It requires four weeks of measurement and one controlled change.<\/p>\n<table style=\"width: 100%; border-collapse: collapse; margin: 18px 0 24px; font-size: 15px; color: #333333;\">\n<thead>\n<tr>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Week<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Action<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Output<\/th>\n<th style=\"background: #273171; color: #ffffff; padding: 12px 14px; text-align: left; font-weight: 600; border: 1px solid #273171;\">Gate to proceed<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">1<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Measure A from the drawing, h from the actual basin, and log ballast mass and position on 20 consecutive molds<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Baseline F and a ballast distribution chart<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">F computed and signed off<\/td>\n<\/tr>\n<tr style=\"background: #F5F5F5;\">\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">2<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Standardise block count\/positions, set clamp pitch \u2264 250 mm, add first-pour sign-off<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Revised work instruction + torque\/mass log<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Two shifts run the same setting<\/td>\n<\/tr>\n<tr>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">3<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Pour 200 molds; measure parting-line fin thickness at four fixed points; plot SPC<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Capability of the new setting<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Fin thickness stable and below limit<\/td>\n<\/tr>\n<tr style=\"background: #F5F5F5;\">\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">4<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Write the eight RFQ fields into the drawing notes and quality agreement; re-audit the flask<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Controlled document + audit record<\/td>\n<td style=\"border: 1px solid #E5E5E5; padding: 10px 14px;\">Supplier accepts measurable limits<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p style=\"margin: 0 0 18px;\">Where simulation is available, use <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/blog\/casting-simulation\/\" target=\"_blank\" rel=\"noopener\">solidification simulation<\/a> to confirm fill sequence and head before changing the basin; where it is not, a physical trial is still cheap. <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/prototipo-de-impressao-3d\/\" target=\"_blank\" rel=\"noopener\">Prot\u00f3tipos impressos em 3D<\/a> let you test a revised projection area without cutting a new pattern. And because extra ballast and longer pouring cycles both carry an energy cost, cross-check the change against <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/blog\/foundry-energy-efficiency\/\" target=\"_blank\" rel=\"noopener\">foundry energy efficiency<\/a> before scaling it across a whole line.<\/p>\n<h2 style=\"font-family: 'Poppins',sans-serif; color: #273171; font-size: 25px; font-weight: 600; line-height: 1.3; margin: 34px 0 14px; padding: 4px 0 4px 30px; background: linear-gradient(to right, #ff512f 0px, #dd2476 5px, transparent 5px);\">Perguntas frequentes<\/h2>\n<h3 style=\"font-family: 'Poppins',sans-serif; color: #273171; font-size: 20px; font-weight: 600; line-height: 1.4; margin: 22px 0 8px;\">Is cope lift the same as core float?<\/h3>\n<p style=\"margin: 0 0 18px;\">No. Core float is the buoyancy of a low-density core immersed in liquid metal, resisted by core prints and chaplets, with net lift proportional to (\u03c1<sub>metal<\/sub> \u2212 \u03c1<sub>core<\/sub>) \u00d7 V<sub>core<\/sub>. Cope lift is pressure on a horizontal projection, \u03c1<sub>metal<\/sub> \u00d7 g \u00d7 h \u00d7 A, resisted by ballast or clamps. See <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/blog\/casting-mold-design-patterns\/\" target=\"_blank\" rel=\"noopener\">mold and pattern design<\/a> for the core calculation.<\/p>\n<h3 style=\"font-family: 'Poppins',sans-serif; color: #273171; font-size: 20px; font-weight: 600; line-height: 1.4; margin: 22px 0 8px;\">Does a heavier casting always need more ballast?<\/h3>\n<p style=\"margin: 0 0 18px;\">No. Uplift depends on projected area and head, not casting mass. A 20 kg thin cover plate can require four times the hold-down of a 105 kg compact boss. Approving ballast by part weight systematically under-protects flat parts; see <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/blog\/casting-price-per-kg\/\" target=\"_blank\" rel=\"noopener\">why mass-based quoting breaks down here<\/a>.<\/p>\n<h3 style=\"font-family: 'Poppins',sans-serif; color: #273171; font-size: 20px; font-weight: 600; line-height: 1.4; margin: 22px 0 8px;\">Can we simply lower the pouring basin to reduce cope lift?<\/h3>\n<p style=\"margin: 0 0 18px;\">Only within the window that filling and feeding allow. Reducing h lowers uplift linearly, but too little head causes misruns and poor feeding. Set the head from <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/blog\/casting-pouring-temperature\/\" target=\"_blank\" rel=\"noopener\">filling and superheat requirements<\/a> e <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/blog\/casting-riser-design\/\" target=\"_blank\" rel=\"noopener\">riser feeding rules<\/a> first, then size the hold-down to that head.<\/p>\n<h3 style=\"font-family: 'Poppins',sans-serif; color: #273171; font-size: 20px; font-weight: 600; line-height: 1.4; margin: 22px 0 8px;\">What safety factor should we specify?<\/h3>\n<p style=\"margin: 0 0 18px;\">Use 1.5 for hand-poured production, 1.8\u20132.0 on automated lines, and add 0.2 when venting is restricted. Apply it to total required resistance, then subtract cope self-weight \u2014 do not simply multiply the ballast mass by the factor.<\/p>\n<h3 style=\"font-family: 'Poppins',sans-serif; color: #273171; font-size: 20px; font-weight: 600; line-height: 1.4; margin: 22px 0 8px;\">How do we tell cope lift from ordinary parting-line flash?<\/h3>\n<p style=\"margin: 0 0 18px;\">A cope lift fin is thick, tapering, and usually heavier near the sprue, often with metal spilled outside the flask. Uniform thin flash points to worn pins or a dirty joint instead. Record the distinction in the <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/blog\/casting-nonconformance\/\" target=\"_blank\" rel=\"noopener\">nonconformance report<\/a> and, if salvage is proposed, treat <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/blog\/casting-weld-repair\/\" target=\"_blank\" rel=\"noopener\">weld repair<\/a> as cosmetic only \u2014 it does not fix the hydrostatic cause. For process comparisons, see <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/blog\/fundicao-em-areia-vs-fundicao-por-cera-perdida\/\" target=\"_blank\" rel=\"noopener\">sand vs investment casting<\/a> e <a style=\"color: #086ad4; text-decoration: none;\" href=\"https:\/\/chinametalfoundry.com\/pt\/fundicao-a-cera-perdida\/\" target=\"_blank\" rel=\"noopener\">fundi\u00e7\u00e3o \u00e0 cera perdida<\/a>, where a ceramic shell has no parting-plane joint to lift.<\/p>\n\t\t<div data-elementor-type=\"section\" data-elementor-id=\"3550\" class=\"elementor elementor-3550\" data-elementor-post-type=\"elementor_library\">\n\t\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-19b1acf1 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"19b1acf1\" data-element_type=\"section\" data-e-type=\"section\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;,&quot;ekit_has_onepagescroll_dot&quot;:&quot;yes&quot;}\">\n\t\t\t\t\t\t\t<div class=\"elementor-background-overlay\"><\/div>\n\t\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-56e26ed6\" data-id=\"56e26ed6\" data-element_type=\"column\" data-e-type=\"column\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-52c3d00c elementor-widget elementor-widget-elementskit-heading\" data-id=\"52c3d00c\" data-element_type=\"widget\" data-e-type=\"widget\" data-settings=\"{&quot;ekit_we_effect_on&quot;:&quot;none&quot;}\" data-widget_type=\"elementskit-heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<div class=\"ekit-wid-con\" ><div class=\"ekit-heading elementskit-section-title-wraper text_left   ekit_heading_tablet-   ekit_heading_mobile-\"><h3 class=\"ekit-heading--title elementskit-section-title\">\u00c0 procura de uma fundi\u00e7\u00e3o de metal fi\u00e1vel na China?<\/h3><\/div><\/div>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-24c75aa0 elementor-widget elementor-widget-text-editor\" data-id=\"24c75aa0\" data-element_type=\"widget\" data-e-type=\"widget\" data-settings=\"{&quot;ekit_we_effect_on&quot;:&quot;none&quot;}\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<ul><li>Podemos ajud\u00e1-lo a otimizar o design de produtos e a poupar custos.<\/li><li>Podemos ajud\u00e1-lo com pe\u00e7as fundidas de alta qualidade e em grandes quantidades.<\/li><li>Podemos entregar a tempo e obter mais oportunidades no mercado de vendas.<\/li><li>Ir\u00e1 beneficiar do servi\u00e7o de fundi\u00e7\u00e3o de metais da Supro MFG.<\/li><\/ul>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-51a20937 elementor-align-left elementor-widget elementor-widget-global elementor-global-1143 elementor-widget-button\" data-id=\"51a20937\" data-element_type=\"widget\" data-e-type=\"widget\" data-settings=\"{&quot;ekit_we_effect_on&quot;:&quot;none&quot;}\" data-widget_type=\"button.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<div class=\"elementor-button-wrapper\">\n\t\t\t\t\t<a class=\"elementor-button elementor-button-link elementor-size-sm elementor-animation-grow\" href=\"https:\/\/chinametalfoundry.com\/pt\/contacto\/\">\n\t\t\t\t\t\t<span class=\"elementor-button-content-wrapper\">\n\t\t\t\t\t\t\t\t\t<span class=\"elementor-button-text\">Pedir um Or\u00e7amento Direto da F\u00e1brica <\/span>\n\t\t\t\t\t<\/span>\n\t\t\t\t\t<\/a>\n\t\t\t\t<\/div>\n\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<\/div>\n\t\t\n<p class=\"sc-note\" style=\"font-size: 13px; color: #9a9a9a; margin: 28px 0 0;\">*Force and cost figures are worked examples computed from stated alloy densities, ASTM A536 \/ ASTM E446 references and Supro MFG shop-floor records. Validate against your own flask geometry, basin height and production volume before specifying ballast.<\/p>\n<\/article>","protected":false},"excerpt":{"rendered":"<p>Cope lift is the failure that looks like a cleaning problem but is actually a hydrostatic calculation. When molten metal [&hellip;]<\/p>\n","protected":false},"author":5,"featured_media":8720,"comment_status":"closed","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"default","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"","ast-breadcrumbs-content":"","ast-featured-img":"","footer-sml-layout":"","ast-disable-related-posts":"","theme-transparent-header-meta":"default","adv-header-id-meta":"","stick-header-meta":"default","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"set","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"var(--ast-global-color-4)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":""},"categories":[51],"tags":[47,49,42,43],"class_list":["post-8718","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-casting-processes","tag-casting-process","tag-manufacturing-process","tag-metal-casting","tag-sand-casting"],"_links":{"self":[{"href":"https:\/\/chinametalfoundry.com\/pt\/wp-json\/wp\/v2\/posts\/8718","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/chinametalfoundry.com\/pt\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/chinametalfoundry.com\/pt\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/chinametalfoundry.com\/pt\/wp-json\/wp\/v2\/users\/5"}],"replies":[{"embeddable":true,"href":"https:\/\/chinametalfoundry.com\/pt\/wp-json\/wp\/v2\/comments?post=8718"}],"version-history":[{"count":6,"href":"https:\/\/chinametalfoundry.com\/pt\/wp-json\/wp\/v2\/posts\/8718\/revisions"}],"predecessor-version":[{"id":8736,"href":"https:\/\/chinametalfoundry.com\/pt\/wp-json\/wp\/v2\/posts\/8718\/revisions\/8736"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/chinametalfoundry.com\/pt\/wp-json\/wp\/v2\/media\/8720"}],"wp:attachment":[{"href":"https:\/\/chinametalfoundry.com\/pt\/wp-json\/wp\/v2\/media?parent=8718"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/chinametalfoundry.com\/pt\/wp-json\/wp\/v2\/categories?post=8718"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/chinametalfoundry.com\/pt\/wp-json\/wp\/v2\/tags?post=8718"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}